AWS B2.1/B2.1M-BMG:2014
Base Metal Grouping for Welding Procedure and Performance Qualification AWS B2.1/B2.1M-BMG:2014
Base Metal Grouping for Welding Procedure and Performance Qualification
3rd Edition
Supersedes AWS B2.1-B2.1M-BMG:2009-ADD1
Prepared by the American Welding Society (AWS) B2 Committee on Procedure and Performance Qualification
Under the Direction of the AWS Technical Activities Committee
Approved by the AWS Board of Directors
Abstract
This document provides the AWS base metal grouping for welding procedure and performance qualification and is identical to Annex C of AWS B2.1/B2.1M:2014, Specification for Welding Procedure and Performance Qualification. AWS B2.1/B2.1M-BMG:2014
ISBN: 978-0-87171-849-5 © 2014 by American Welding Society All rights reserved Printed in the United States of America
Photocopy Rights. No portion of this standard may be reproduced, stored in a retrieval system, or transmitted in any form, including mechanical, photocopying, recording, or otherwise, without the prior written permission of the copyright owner. Authorization to photocopy items for internal, personal, or educational classroom use only or the internal, personal, or educational classroom use only of specific clients is granted by the American Welding Society provided that the appropriate fee is paid to the Copyright Clearance Center, 222 Rosewood Drive, Danvers, MA 01923, tel: (978) 750-8400; Internet:
ii AWS B2.1/B2.1M-BMG:2014
Statement on the Use of American Welding Society Standards All standards (codes, specifications, recommended practices, methods, classifications, and guides) of the American Welding Society (AWS) are voluntary consensus standards that have been developed in accordance with the rules of the American National Standards Institute (ANSI). When AWS American National Standards are either incorporated in, or made part of, documents that are included in federal or state laws and regulations, or the regulations of other govern- mental bodies, their provisions carry the full legal authority of the statute. In such cases, any changes in those AWS standards must be approved by the governmental body having statutory jurisdiction before they can become a part of those laws and regulations. In all cases, these standards carry the full legal authority of the contract or other document that invokes the AWS standards. Where this contractual relationship exists, changes in or deviations from requirements of an AWS standard must be by agreement between the contracting parties. AWS American National Standards are developed through a consensus standards development process that brings together volunteers representing varied viewpoints and interests to achieve consensus. While AWS administers the process and establishes rules to promote fairness in the development of consensus, it does not independently test, evalu- ate, or verify the accuracy of any information or the soundness of any judgments contained in its standards. AWS disclaims liability for any injury to persons or to property, or other damages of any nature whatsoever, whether special, indirect, consequential, or compensatory, directly or indirectly resulting from the publication, use of, or reliance on this standard. AWS also makes no guarantee or warranty as to the accuracy or completeness of any information published herein. In issuing and making this standard available, AWS is neither undertaking to render professional or other services for or on behalf of any person or entity, nor is AWS undertaking to perform any duty owed by any person or entity to someone else. Anyone using these documents should rely on his or her own independent judgment or, as appropriate, seek the advice of a competent professional in determining the exercise of reasonable care in any given circumstances. It is assumed that the use of this standard and its provisions is entrusted to appropriately qualified and competent personnel. This standard may be superseded by new editions. This standard may also be corrected through publication of amendments or errata or supplemented by publication of addenda. Information on the latest editions of AWS standards including amendments, errata, and addenda is posted on the AWS web page (www.aws.org). Users should ensure that they have the latest edition, amendments, errata, and addenda. Publication of this standard does not authorize infringement of any patent or trade name. Users of this standard accept any and all liabilities for infringement of any patent or trade name items. AWS disclaims liability for the infringement of any patent or product trade name resulting from the use of this standard. AWS does not monitor, police, or enforce compliance with this standard, nor does it have the power to do so. Official interpretations of any of the technical requirements of this standard may only be obtained by sending a request, in writing, to the appropriate technical committee. Such requests should be addressed to the American Welding Society, Attention: Managing Director, Technical Services Division, 8669 NW 36 St, # 130, Miami, FL 33166. With regard to technical inquiries made concerning AWS standards, oral opinions on AWS standards may be rendered. These opinions are offered solely as a convenience to users of this standard, and they do not constitute professional advice. Such opinions represent only the personal opinions of the particular individuals giving them. These individuals do not speak on behalf of AWS, nor do these oral opinions constitute official or unofficial opinions or interpretations of AWS. In addition, oral opinions are informal and should not be used as a substitute for an official interpretation. This standard is subject to revision at any time by the AWS required and should be addressed to AWS Headquarters. Such comments will receive careful consideration by the AWS B2 Committee on Procedure and Performance Qualification. It must be reviewed every five years, and if not revised, it must be either reaffirmed or withdrawn. Comments (recom- mendations, additions, or deletions) and any pertinent data that may be of use in improving this standard are required and should be addressed to AWS Headquarters. Such comments will receive careful consideration by the AWS B2 Committee on Procedure and Performance Qualification and the author of the comments will be informed of the Committee’s response to the comments. Guests are invited to attend all meetings of the AWS required and should be addressed to AWS Headquarters. Such comments will receive careful consideration by the AWS B2 Committee on Procedure and Performance Qualification to express their comments verbally. Procedures for appeal of an adverse decision concerning all such comments are provided in the Rules of Operation of the Technical Activities Committee. A copy of these Rules can be obtained from the American Welding Society, 8669 NW 36 St, # 130, Miami, FL 33166.
iii AWS B2.1/B2.1M-BMG:2014
This page is intentionally blank.
iv AWS B2.1/B2.1M-BMG:2014
Personnel
AWS B2 Committee on Procedure and Performance Qualification J. J. Fluckiger, Chair Idaho National Laboratory J. L. Cooley, 1st Vice Chair J. C. & Associates, Incorporated E. W. Beckman, 2nd Vice Chair Consultant A. L. Diaz, Secretary American Welding Society D. M. Allbritten GE Capital M. Bernasek C-SPEC K. L. Bingham Los Alamos National Laboratory H. R. Castner Edison Welding Institute D. W. Craig Computer Engineering, Incorporated E. H. Gray U.S. Nuclear Regulatory Commission M. F. Herrle Arise K. G. Kofford Idaho National Laboratory R. A. LaFave Consultant G. S. Michels Summit Consulting A. S. Olivares HSB Global Standards J. F. Pike NASA Langley Research Center W. M. Ruof Bechtel Plant Machinery, Incorporated J. J. Sekely Welding Services, Incorporated M. R. Stone URS Flint M. L. Thomas Rocky Mountain Testing, LLC G. M. Wisbrock, Jr. Consultant R. K. Wiswesser Welder Training & Testing Institute
Advisors to the AWS B2 Committee on Procedure and Performance Qualification L. P. Connor Consultant W. D. Doty Doty & Associates, Incorporated B. J. Hable Ford Motor Company K. Y. Lee U.S. Department of Transportation B. B. MacDonald Consultant F. A. Schweighardt Air Liquide Industrial U.S. LP A. W. Sindel Alstom Power Steam C. E. Spaeder, Jr. Consultant W. J. Sperko Sperko Engineering Services, Incorporated R. F. Waite Consultant
AWS B2B Subcommittee on Welding Qualification M. R. Stone, Chair URS Flint A. L. Diaz, Secretary American Welding Society D. M. Allbritten GE Capital E. W. Beckman Consultant M. Bernasek C-SPEC K. L. Bingham Los Alamos National Laboratory J. L. Cooley J. C. & Associates, Incorporated D. W. Craig Computer Engineering, Incorporated
v AWS B2.1/B2.1M-BMG:2014
AWS B2B Subcommittee on Welding Qualification (Continued) J. J. Fluckiger Idaho National Laboratory E. H. Gray U.S. Nuclear Regulatory Commission K. G. Kofford Idaho National Laboratory G. S. Michels Summit Consulting A. S. Olivares HSB Global Standards J. F. Pike NASA Langley Research Center J. J. Sekely Welding Services, Incorporated M. L. Thomas Rocky Mountain Testing, LLC G. M. Wisbrock Jr. Consultant R. K. Wiswesser Welder Training & Testing Institute
Advisors to the AWS B2B Subcommittee on Welding Qualification L. P. Connor Consultant W. D. Doty Doty & Associates, Incorporated J. G. Feldstein Foster Wheeler North America B. J. Hable Ford Motor Company K. Y. Lee U.S. Department of Transportation A. W. Sindel Alstom Power Steam W. J. Sperko Sperko Engineering Service, Incorporated
AWS B2C Subcommittee on Materials W. M. Ruof, Chair Bechtel Plant Machinery Incorporated A. L. Diaz, Secretary American Welding Society M. Bernasek C-SPEC J. J. Fluckiger Idaho National Laboratory M. F. Herrle Arise K. G. Kofford Idaho National Laboratory R. A. LaFave Consultant
Advisors to the AWS B2C Subcommittee on Materials C. E. Cross Los Alamos National Laboratory A. Donlevy International Titanium Association W. D. Doty Doty & Associates, Incorporated P. Pollak Pollak & Associates A. W. Sindel Alstom Power Steam C. E. Spaeder, Jr. Consultant L. T. Vernam AlcoTec Wire Corporation G. M. Wisbrock, Jr. Consultant
vi AWS B2.1/B2.1M-BMG:2014
Table of Contents
Page No. Personnel ...... v List of Tables...... vii 1. Scope ...... 1 Annex C—Base Metal Grouping ...... 3
List of Tables
Table Page No. C.1 Listing of Base Metal Specifications—Ferrous Alloys ...... 4 C.1 Listing of Base Metal Specifications—Nonferrous Alloys ...... 54 C.2 M-Number Listing of Base Metals—Ferrous Alloys...... 82 C.2 M-Number Listing of Base Metals—Nonferrous Alloys...... 155 C.3 Listing of Base Metal Specifications—Iron Castings...... 204
vii AWS B2.1/B2.1M-BMG:2014
This page is intentionally blank.
viii AWS B2.1/B2.1M-BMG:2014
Base Metal Grouping for Welding Procedure and Performance Qualification
1. Scope This publication is an extract of AWS B2.1/B2.1M:2014, Specification for Welding Procedure and Performance Qualifi- cation, and is identical to Annex C, Base Metal Grouping, in the 2014 edition of that standard. This publication super- sedes AWS B2.1/B2.1M-BMG:2009-ADD1. Underlined text or a vertical line in the margin indicates a revision from the 2009 edition. This publication may be referred to by other codes and standards that have welding procedure and performance require- ments in order to avoid duplication of materials tables in those publications. Base metals and filler metals have been grouped into categories that will minimize the number of qualification tests required. Substitution of one base metal or filler metal for another, even when within the allowable rules, should only be made after an evaluation of the factors involved. For some materials, additional tests may be required. Materials not listed require separate qualification.
1 AWS B2.1/B2.1M-BMG:2014
This page is intentionally blank.
2 AWS B2.1/B2.1M-BMG:2014
Annex C (Normative) Base Metal Grouping (see 3, 4.3.12, 4.3.15, and Table 5.3)
This annex is part of AWS B2.1/B2.1M-BMG:2014, Base Metal Grouping for Welding Procedure and Performance Qualification, and includes mandatory elements for use with this standard.
C1. Base Metal Specifications Table C.1 indexes ASTM, ABS, API, AS, AS/NZS, CSA, AMS, ISO, NACE, and MSS base metals in numerical order to provide ease of reference when determining into what grouping a particular base metal specification falls. Table C.2 groups base metals for welding procedure and performance qualification on the basis of mechanical proper- ties, chemical composition, and metallurgical compatibility to minimize the number of welding qualification where this can logically be done. Table C.3 lists base metal specifications for iron castings in accordance with AWS D11.2 groups.
C2. Material Number (M-Number) Groupings Base metal has been divided into general categories, e.g., Material Numbers (M-Numbers) 1, 1A, 3, 3A, 4, 4A, etc., and further divided into groups within each general category. The category grouping does not imply that base metals may be substituted for other base metals within the same Mate- rial Number (M-Number) without consideration for weldability.
C3. Iron Castings Specifications Base metal specifications for iron castings are divided into D11.2 groups.
3 AWS B2.1/B2.1M-BMG:2014
Table C.1 List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys AAR M201 1 1 11.1 A — Castings AAR M201 1 2 11.1 B — Castings AAR M201 1 3 11.1 B+ — Castings AAR M201 1 4 11.1 C — Castings AAR TC128 10C 1 11.1 B — Plate ABS ABS 1 1 1.1 E K01801 Plate, Bar, & Shapes ABS ABS 1 1 1.1 D K02101 Plate, Bar, & Shapes ABS ABS 1 1 1.1 B K02102 Plate, Bar, & Shapes ABS ABS 1 1 1.1 A K02300 Plate, Bar, & Shapes ABS ABS 1 1 1.2 AH32 K11846 Plate, Bar, & Shapes ABS ABS 1 1 1.2 DH32 K11846 Plate, Bar, & Shapes ABS ABS 1 1 1.2 EH32 K11846 Plate, Bar, & Shapes ABS ABS 1 1 1.2 FH32 K11846 Plate, Bar, & Shapes ABS ABS 1 2 1.2 AH36 K11852 Plate, Bar, & Shapes ABS ABS 1 2 1.2 DH36 K11852 Plate, Bar, & Shapes ABS ABS 1 2 1.2 EH36 K11852 Plate, Bar, & Shapes ABS ABS 1 2 1.2 FH36 K11852 Plate, Bar, & Shapes ABS ABS 1 2 1.3 AH40 K11857 Plate, Bar, & Shapes ABS ABS 1 2 1.3 DH40 K11857 Plate, Bar, & Shapes ABS ABS 1 2 1.3 EH40 K11857 Plate, Bar, & Shapes ABS ABS 1 2 1.3 FH40 K11857 Plate, Bar, & Shapes API 2H 1 1 1.2 42 — Plate API 2H 1 2 1.2 50 — Plate API 2MT1 1 1 1.2 50 — Plate API 2W 1 1 1.2 50 — Plate API 2W 1 2 1.3 60 — Plate API 2Y 1 1 1.2 42 — Plate API 2Y 1 1 1.2 50 — Plate API 2Y 1 2 1.2 50T — Plate API 2Y 1 2 1.3 60 — Plate API 5L 1 1 1.1 A — Seamless & Welded Pipe API 5L 1 1 1.1 A25 — Seamless & Welded Pipe API 5L 1 1 1.1 A25, Cl. I — Seamless & Welded Pipe & Tube API 5L 1 1 1.1 A25, Cl. II — Seamless & Welded Pipe & Tube API 5L 1 1 1.1 A25P — Seamless & Welded Pipe API 5L 1 1 11.1 B — Seamless & Welded Pipe API 5L 1 1 1.1 BM — Welded Pipe API 5L 1 1 1.1 BMO — Welded Pipe API 5L 1 1 1.1 BMS — Welded Pipe API 5L 1 1 1.1 BN — Seamless & Welded Pipe API 5L 1 1 1.1 BNO — Seamless & Welded Pipe API 5L 1 1 1.1 BNS — Seamless & Welded Pipe
(Continued)
4 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys API 5L 1 1 1.1 BQ — Seamless & Welded Pipe API 5L 1 1 1.1 BQO — Seamless & Welded Pipe API 5L 1 1 1.1 BQS — Seamless & Welded Pipe API 5L 1 1 1.1 BR — Seamless & Welded Pipe API 5L 1 1 11.1 X42 — Seamless & Welded Pipe API 5L 1 1 1.2 X42M — Welded Pipe API 5L 1 1 1.2 X42MO — Welded Pipe API 5L 1 1 1.2 X42MS — Welded Pipe API 5L 1 1 1.2 X42N — Seamless & Welded Pipe API 5L 1 1 1.2 X42NO — Seamless & Welded Pipe API 5L 1 1 1.2 X42NS — Seamless & Welded Pipe API 5L 1 1 1.2 X42Q — Seamless & Welded Pipe API 5L 1 1 1.2 X42QO — Seamless & Welded Pipe API 5L 1 1 1.2 X42QS — Seamless & Welded Pipe API 5L 1 1 1.2 X42R — Seamless & Welded Pipe API 5L 1 1 11.1 X46 — Seamless & Welded Pipe API 5L 1 1 1.2 X46M — Welded Pipe API 5L 1 1 1.2 X46MO — Welded Pipe API 5L 1 1 1.2 X46MS — Welded Pipe API 5L 1 1 1.2 X46N — Seamless & Welded Pipe API 5L 1 1 1.2 X46NO — Seamless & Welded Pipe API 5L 1 1 1.2 X46NS — Seamless & Welded Pipe API 5L 1 1 1.2 X46Q — Seamless & Welded Pipe API 5L 1 1 1.2 X46QO — Seamless & Welded Pipe API 5L 1 1 1.2 X46QS — Seamless & Welded Pipe API 5L 1 1 11.1 X52 — Seamless & Welded Pipe API 5L 1 1 1.2 X52M — Welded Pipe API 5L 1 1 1.2 X52MO — Welded Pipe API 5L 1 1 1.2 X52MS — Welded Pipe API 5L 1 1 1.2 X52N — Seamless & Welded Pipe API 5L 1 1 1.2 X52NO — Seamless & Welded Pipe API 5L 1 1 1.2 X52NS — Seamless & Welded Pipe API 5L 1 1 1.2 X52Q — Seamless & Welded Pipe API 5L 1 1 1.2 X52QO — Seamless & Welded Pipe API 5L 1 1 1.2 X52QS — Seamless & Welded Pipe API 5L 1 2 11.1 X56 — Seamless & Welded Pipe API 5L 1 2 2.1 X56M — Welded Pipe API 5L 1 2 2.1 X56MO — Welded Pipe API 5L 1 2 2.1 X56MS — Welded Pipe API 5L 1 2 1.3 X56N — Seamless & Welded Pipe API 5L 1 2 3.1 X56Q — Seamless & Welded Pipe API 5L 1 2 3.1 X56QO — Seamless & Welded Pipe
(Continued)
5 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys API 5L 1 2 3.1 X56QS — Seamless & Welded Pipe API 5L 1 2 11.1 X60 — Seamless & Welded Pipe API 5L 1 2 2.1 X60M — Welded Pipe API 5L 1 2 2.1 X60MO — Welded Pipe
API 5L 1 2 2.1 X60MS — Welded Pipe API 5L 1 2 1.3 X60N — Seamless & Welded Pipe API 5L 1 2 3.1 X60Q — Seamless & Welded Pipe API 5L 1 2 3.1 X60QO — Seamless & Welded Pipe API 5L 1 2 3.1 X60QS — Seamless & Welded Pipe API 5L 1 2 11.1 X65 — Seamless & Welded Pipe API 5L 1 2 2.1 X65M — Welded Pipe API 5L 1 2 2.1 X65MO — Welded Pipe API 5L 1 2 2.1 X65MS — Welded Pipe API 5L 1 2 3.1 X65Q — Seamless & Welded Pipe API 5L 1 2 3.1 X65QO — Seamless & Welded Pipe API 5L 1 2 3.1 X65QS — Seamless & Welded Pipe API 5L 1 3 11.1 X70 — Seamless & Welded Pipe API 5L 1 3 2.2 X70M — Welded Pipe API 5L 1 3 2.2 X70MO — Welded Pipe API 5L 1 3 2.2 X70MS — Welded Pipe API 5L 1 3 3.1 X70Q — Seamless & Welded Pipe API 5L 1 3 3.1 X70QO — Seamless & Welded Pipe API 5L 1 3 3.1 X70QS — Seamless & Welded Pipe API 5L 1 4 2.2 X80M — Welded Pipe API 5L 1 4 2.2 X80MO — Welded Pipe API 5L 1 4 3.1 X80Q — Seamless & Welded Pipe API 5L 1 4 3.1 X80QO — Seamless & Welded Pipe API 5LS 1 1 11.1 X46 — Spiral Welded Pipe AS ASTM A945 1 2 1.2 50 — Plate AS ASTM A945 1 2 1.3 65 — Plate AS 1548 1 2 1.2 5-490 — Plate AS 1548 1 1 1.2 7-430 — Plate AS 1548 1 1 1.2 7-460 — Plate AS 1548 1 2 1.2 7-490 — Plate AS 1548 1 1 1.2 PT430 — Plate AS 1548 1 1 1.2 PT460 — Plate AS 1548 1 2 1.2 PT490 — Plate AS/NZS 1594 1 1 1.1 HA1 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.1 HA200 — Plate, Sheet, & Strip
(Continued)
6 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys AS/NZS 1594 1 1 1.1 HA250 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.1 HA250/1 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.1 HA3 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.2 HA300 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.2 HA300/1 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.2 HA350 — Plate, Sheet, & Strip AS/NZS 1594 1 1 2.1 HA400 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.1 HA4N — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.1 HU250 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.2 HU300 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.2 HU300/1 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.4 HW350 — Plate, Sheet, & Strip AS/NZS 1594 1 1 1.2 XF300 — Plate, Sheet, & Strip AS/NZS 1594 1 1 2.1 XF400 — Plate, Sheet, & Strip AS/NZS 1594 1 3 2.2 XF500 — Plate, Sheet, & Strip AS/NZS 3597 11B — 3.1 700PV — Plate AS/NZS 3678 1 1 1.1 200 — Plate AS/NZS 3678 1 1 1.2 250 — Plate AS/NZS 3678 1 1 1.2 250L15 — Plate AS/NZS 3678 1 2 1.2 300 — Plate AS/NZS 3678 1 2 1.2 300L15 — Plate AS/NZS 3678 1 2 1.2 350 — Plate AS/NZS 3678 1 2 1.2 350L15 — Plate AS/NZS 3678 1 2 1.3 400 — Plate AS/NZS 3678 1 2 1.3 400L15 — Plate AS/NZS 3678 1 2 1.3 450 — Plate AS/NZS 3678 1 2 1.3 450L15 — Plate AS/NZS 3678 3 1 1.4 WR350 — Plate AS/NZS 3678 3 1 1.4 WR350L0 — Plate AS/NZS 3679.1 1 1 1.1 250 — Bar & Sections AS/NZS 3679.1 1 1 1.1 250L0 — Bar & Sections AS/NZS 3679.1 1 1 1.1 250L15 — Bar & Sections AS/NZS 3679.1 1 2 1.2 300 — Bar & Sections AS/NZS 3679.1 1 2 1.2 300L0 — Bar & Sections AS/NZS 3679.1 1 2 1.2 300L15 — Bar & Sections AS/NZS 3679.1 1 2 1.2 350 — Bar & Sections AS/NZS 3679.1 1 2 1.2 350L0 — Bar & Sections AS/NZS 3679.1 1 2 1.2 350L15 — Bar & Sections AS/NZS 3679.1 1 2 1.3 400 — Bar & Sections AS/NZS 3679.1 1 2 1.3 400L0 — Bar & Sections AS/NZS 3679.1 1 2 1.3 400L15 — Bar & Sections ASTM A27 1 1 11.1 60-30 J03000 Castings
(Continued)
7 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A27 1 1 11.1 65-35 J03001 Castings ASTM A27 1 2 11.1 70-36 J03501 Castings ASTM A27 1 2 1.1 70-40 J02501 Castings ASTM A27 1 1 1.1 U-60-30 J03000 Castings ASTM/ASME A/SA-31 1 1 11.1 B K03100 Rivets ASTM/ASME A/SA-36 1 1 11.1 — — Bar ASTM/ASME A/SA-36 1 1 11.1 — K02595 Plates ASTM/ASME A/SA-36 1 1 11.1 — K02596 Plates ASTM/ASME A/SA-36 1 1 11.1 — K02597 Plates ASTM/ASME A/SA-36 1 1 1.1 — K02598 Plates ASTM/ASME A/SA-36 1 1 1.1 — K02599 Plates ASTM/ASME A/SA-36 1 1 11.1 — K02600 Shapes ASTM/ASME A/SA-53 1 1 1.1 E, A K02504 Resistance Welded Pipe ASTM/ASME A/SA-53 1 1 11.1 E, B K03005 Resistance Welded Pipe ASTM/ASME A/SA-53 1 1 11.1 F K03005 Furnace Welded Pipe ASTM/ASME A/SA-53 1 1 1.1 S, A K02504 Seamless Pipe ASTM/ASME A/SA-53 1 1 11.1 S, B K03005 Seamless Pipe ASTM/ASME A/SA-105 1 2 11.1 — K03504 Flanges & Fittings ASTM/ASME A/SA-106 1 1 1.1 A K02501 Seamless Pipe ASTM/ASME A/SA-106 1 1 11.1 B K03006 Seamless Pipe ASTM/ASME A/SA-106 1 2 11.1 C K03501 Seamless Pipe ASTM A108 1 1 1.1 1015 CW G10150 Bar ASTM A108 1 1 1.1 1018 CW G10180 Bar ASTM A108 1 1 1.1 1020 CW G10200 Bar ASTM A108 3 3 4.1 8620 CW G86200 Bar ASTM A131 1 1 1.1 A — Plate, Shapes, Bar, & Rivets ASTM A131 1 2 1.2 AH32 — Plate, Shapes, Bar, & Rivets ASTM A131 1 2 1.2 AH36 — Plate, Shapes, Bar, & Rivets ASTM A131 1 1 1.1 B — Plate, Shapes, Bar, & Rivets ASTM A131 1 1 1.1 CS — Plate, Shapes, Bar, & Rivets ASTM A131 1 1 1.1 D — Plate, Shapes, Bar, & Rivets ASTM A131 1 2 1.2 DH32 — Plate, Shapes, Bar, & Rivets ASTM A131 1 2 1.2 DH36 — Plate, Shapes, Bar, & Rivets ASTM A131 1 1 1.1 DS — Plate, Shapes, Bar, & Rivets ASTM A131 1 2 1.1 E — Plate, Shapes, Bar, & Rivets ASTM A131 1 2 1.2 EH32 — Plate, Shapes, Bar, & Rivets ASTM A131 1 2 1.2 EH36 — Plate, Shapes, Bar, & Rivets ASTM/ASME A/SA-134 1 1 1.1 SA283, A K01400 Welded Pipe ASTM/ASME A/SA-134 1 1 1.1 SA283, B K01702 Welded Pipe ASTM/ASME A/SA-134 1 1 1.1 SA283, C K02401 Welded Pipe ASTM/ASME A/SA-134 1 1 11.1 SA283, D K02702 Welded Pipe ASTM/ASME A/SA-134 1 1 1.1 SA285, A K01700 Welded Pipe
(Continued)
8 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-134 1 1 1.1 SA285, B K02200 Welded Pipe ASTM/ASME A/SA-134 1 1 11.1 SA285, C K02801 Welded Pipe ASTM/ASME A/SA-134 1 1 1.1 SA36 K02599 Welded Pipe ASTM/ASME A/SA-135 1 1 1.1 A K02509 E.R.W. Pipe ASTM/ASME A/SA-135 1 1 11.1 B K03018 E.R.W. Pipe ASTM A139 1 1 1.1 A K02508 Welded Pipe ASTM A139 1 1 11.1 B K03003 Welded Pipe ASTM A139 1 1 11.1 C K03004 Welded Pipe ASTM A139 1 1 11.1 D K03010 Welded Pipe ASTM A139 1 1 11.1 E K03012 Welded Pipe ASTM A148 4 3 — 90-60 D50600 Castings ASTM A161 1 1 — Low Carbon K01504 Tube ASTM A161 3 1 1.1 T1 K11522 Tube ASTM A167 8 1 8.1 302B S30215 Plate, Sheet, & Strip ASTM A167 8 2 8.2 308 S30800 Plate, Sheet, & Strip ASTM A167 8 2 8.2 309 S30900 Plate, Sheet, & Strip ASTM A167 8 2 8.2 310 S31000 Plate, Sheet, & Strip ASTM/ASME A/SA-178 1 1 1.1 A K01200 E.R.W. Tube ASTM/ASME A/SA-178 1 1 11.1 C K03503 E.R.W. Tube ASTM/ASME A/SA-178 1 2 11.1 D K02709 E.R.W. Tube ASTM/ASME A/SA-179 1 1 1.1 — K01200 Seamless Tube ASTM/ASME A/SA-181 1 1 11.1 Cl. 60 K03502 Pipe Flange & Fittings ASTM/ASME A/SA-181 1 2 11.1 Cl. 70 K03502 Pipe Flange & Fittings ASTM/ASME A/SA-182 8 4 8.2 — S32053 Forgings ASTM/ASME A/SA-182 10H 1 10.1 — S32202 Forgings ASTM/ASME A/SA-182 3 2 1.1 F1 K12822 Forgings ASTM/ASME A/SA-182 8 2 8.1 F10 S33100 Forgings ASTM/ASME A/SA-182 4 1 5.1 F11, Cl. 1 K11597 Forgings ASTM/ASME A/SA-182 4 1 5.1 F11, Cl. 2 K11572 Forgings ASTM/ASME A/SA-182 4 1 5.1 F11, Cl. 3 K11572 Forgings ASTM/ASME A/SA-182 4 1 5.1 F12, Cl. 1 K11562 Forgings ASTM/ASME A/SA-182 4 1 5.1 F12, Cl. 2 K11564 Forgings ASTM/ASME A/SA-182 3 2 4.2 F2 K12122 Forgings ASTM/ASME A/SA-182 5A 1 5.2 F21 K31545 Forgings ASTM/ASME A/SA-182 5A 1 5.2 F22, Cl. 1 K21590 Forgings ASTM/ASME A/SA-182 5A 1 5.2 F22, Cl. 3 K21590 Forgings ASTM/ASME A/SA-182 5C 1 6.2 F22V K31835 Forgings ASTM/ASME A/SA-182 8 1 8.1 F304 S30400 Forgings ASTM/ASME A/SA-182 8 1 8.1 F304 S30400 Forgings ASTM/ASME A/SA-182 8 1 8.1 F304H S30409 Forgings ASTM/ASME A/SA-182 8 1 8.1 F304H S30409 Forgings ASTM/ASME A/SA-182 8 1 8.1 F304L S30403 Forgings
(Continued)
9 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-182 8 1 8.1 F304L S30403 Forgings ASTM/ASME A/SA-182 8 1 8.1 F304LN S30453 Forgings ASTM/ASME A/SA-182 8 1 8.1 F304LN S30453 Forgings ASTM/ASME A/SA-182 8 1 8.1 F304N S30451 Forgings ASTM/ASME A/SA-182 8 2 8.2 F310 S31000 Forgings ASTM/ASME A/SA-182 8 2 8.2 F310 S31000 Forgings ASTM/ASME A/SA-182 8 2 8.2 F310MoLN S31050 Forgings ASTM/ASME A/SA-182 8 1 8.1 F316 S31600 Forgings ASTM/ASME A/SA-182 8 1 8.1 F316 S31600 Forgings ASTM/ASME A/SA-182 8 1 8.1 F316H S31609 Forgings ASTM/ASME A/SA-182 8 1 8.1 F316H S31609 Forgings ASTM/ASME A/SA-182 8 1 8.1 F316L S31603 Forgings ASTM/ASME A/SA-182 8 1 8.1 F316L S31603 Forgings ASTM/ASME A/SA-182 8 1 8.1 F316LN S31653 Forgings ASTM/ASME A/SA-182 8 1 8.1 F316LN S31653 Forgings ASTM/ASME A/SA-182 8 1 8.1 F316N S31651 Forgings ASTM/ASME A/SA-182 8 1 8.1 F317 S31700 Forgings ASTM/ASME A/SA-182 8 1 8.1 F317 S31700 Forgings ASTM/ASME A/SA-182 8 1 8.1 F317L S31703 Forgings ASTM/ASME A/SA-182 8 1 8.1 F317L S31703 Forgings ASTM/ASME A/SA-182 8 1 8.1 F321 S32100 Forgings ASTM/ASME A/SA-182 8 1 8.1 F321 S32100 Forgings ASTM/ASME A/SA-182 8 1 8.1 F321H S32109 Forgings ASTM/ASME A/SA-182 8 1 8.1 F321H S32109 Forgings ASTM/ASME A/SA-182 8 1 8.1 F347 S34700 Forgings ASTM/ASME A/SA-182 8 1 8.1 F347 S34700 Forgings ASTM/ASME A/SA-182 8 1 8.1 F347H S34709 Forgings ASTM/ASME A/SA-182 8 1 8.1 F347H S34709 Forgings ASTM/ASME A/SA-182 8 1 8.1 F348 S34800 Forgings ASTM/ASME A/SA-182 8 1 8.1 F348 S34800 Forgings ASTM/ASME A/SA-182 8 1 8.1 F348H S34809 Forgings ASTM/ASME A/SA-182 8 1 8.1 F348H S34809 Forgings ASTM/ASME A/SA-182 5C 1 6.2 F3V K31830 Forgings ASTM/ASME A/SA-182 5C 1 6.2 F3VCb K31390 Forgings ASTM/ASME A/SA-182 6 2 7.2 F429 S42900 Forgings ASTM/ASME A/SA-182 7 2 7.1 F430 S43000 Forgings ASTM/ASME A/SA-182 8 4 8.2 F44 S31254 Forgings ASTM/ASME A/SA-182 8 2 8.2 F45 S30815 Forgings ASTM/ASME A/SA-182 8 1 8.1 F46 S30600 Forgings ASTM/ASME A/SA-182 8 4 8.3 F49 S34565 Forgings ASTM/ASME A/SA-182 5B 1 5.3 F5 K41545 Forgings ASTM/ASME A/SA-182 10H 1 10.2 F50 S31200 Forgings
(Continued)
10 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-182 10H 1 10.1 F51 S31803 Forgings ASTM/ASME A/SA-182 10H 1 10.2 F53 S32750 Forgings ASTM/ASME A/SA-182 10H 1 10.2 F54 S39274 Forgings ASTM/ASME A/SA-182 10H 1 10.1 F55 S32760 Forgings ASTM/ASME A/SA-182 5B 1 5.3 F5a K42544 Forgings ASTM/ASME A/SA-182 10H 1 10.1 F60 S32205 Forgings ASTM/ASME A/SA-182 10H 1 10.2 F61 S32550 Forgings ASTM/ASME A/SA-182 6 1 7.2 F6a, Cl. 1 S41000 Forgings ASTM/ASME A/SA-182 6 3 7.2 F6a, Cl. 2 S41000 Forgings ASTM/ASME A/SA-182 6 3 7.2 F6a, Cl. 3 S41000 Forgings ASTM/ASME A/SA-182 6 3 7.2 F6a, Cl. 4 S41000 Forgings ASTM/ASME A/SA-182 6 3 7.2 F6b S41026 Forgings ASTM/ASME A/SA-182 6 4 7.2 F6NM S41500 Forgings ASTM/ASME A/SA-182 5B 1 5.4 F9 K90941 Forgings ASTM/ASME A/SA-182 15E 1 6.4 F91 K90901 Forgings ASTM/ASME A/SA-182 15E 1 6.4 F92 K92460 Forgings ASTM/ASME A/SA-182 9A 1 9.1 FR K22035 Forgings ASTM/ASME A/SA-182 8 3 8.3 FXM-11 S21904 Forgings ASTM/ASME A/SA-182 8 3 8.3 FXM-19 S20910 Forgings ASTM/ASME A/SA-182 10I 1 7.1 FXM-27Cb S44627 Forgings ASTM/ASME A/SA-192 1 1 1.1 — K01201 Seamless Tube ASTM A199 4 1 5.1 T11 K11597 Seamless Tube ASTM A199 5A 1 — T21 K31545 Seamless Tube ASTM A199 5A 1 5.2 T22 K21590 Seamless Tube ASTM A199 5A 1 — T4 K31509 Seamless Tube ASTM A199 5B 1 5.3 T5 K41545 Seamless Tube ASTM A199 5B 1 5.4 T9 K81590 Seamless Tube ASTM A199 15E 1 6.4 T91 K90901 Seamless Tube ASTM A200 5A 1 — T21 K31545 Tube ASTM A200 5A 1 5.2 T22 K21590 Tube ASTM A200 5A 1 — T4 K31509 Tube ASTM/ASME A/SA-202 4 1 4.2 A K11742 Plate ASTM/ASME A/SA-202 4 1 4.2 B K12542 Plate ASTM/ASME A/SA-203 9A 1 9.1 A K21703 Plate ASTM/ASME A/SA-203 9A 1 9.1 B K22103 Plate ASTM/ASME A/SA-203 9B 1 9.2 D K31718 Plate ASTM/ASME A/SA-203 9B 1 9.2 E K32018 Plate ASTM/ASME A/SA-203 9B 1 9.2 F — Plate ASTM/ASME A/SA-203 9B 1 9.2 F — Plate ASTM/ASME A/SA-204 3 1 1.1 A K11820 Plate ASTM/ASME A/SA-204 3 2 1.1 B K12020 Plate ASTM/ASME A/SA-204 3 2 1.2 C K12320 Plate
(Continued)
11 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-209 3 1 1.1 T1 K11522 Seamless Tube ASTM/ASME A/SA-209 3 1 1.1 T1a K12023 Seamless Tube ASTM/ASME A/SA-209 3 1 1.1 T1b K11422 Seamless Tube ASTM/ASME A/SA-210 1 1 11.1 A-1 K02707 Seamless Tube ASTM/ASME A/SA-210 1 2 11.1 C K03501 Seamless Tube ASTM A211 1 1 1.1 A570-30 K02502 Welded Pipe ASTM A211 1 1 1.1 A570-33 K02502 Welded Pipe ASTM A211 1 1 1.1 A570-40 K02502 Welded Pipe ASTM/ASME A/SA-213 8 2 8.2 310 S31000 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 S30815 S30815 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 S32615 S32615 Seamless Tube ASTM/ASME A/SA-213 8 4 8.3 S34565 S34565 Seamless Tube ASTM/ASME A/SA-213 4 1 5.1 T11 K11597 Seamless Tube ASTM/ASME A/SA-213 4 1 5.1 T12 K11562 Seamless Tube ASTM/ASME A/SA-213 10B 1 4.1 T17 K12047 Seamless Tube ASTM/ASME A/SA-213 3 1 4.2 T2 K11547 Seamless Tube ASTM/ASME A/SA-213 5A 1 5.2 T21 K31545 Seamless Tube ASTM/ASME A/SA-213 5A 1 5.2 T22 K21590 Seamless Tube ASTM/ASME A/SA-213 5B 1 5.3 T5 K41545 Seamless Tube ASTM/ASME A/SA-213 5B 1 5.3 T5b K51545 Seamless Tube ASTM/ASME A/SA-213 5B 1 5.3 T5c K41245 Seamless Tube ASTM/ASME A/SA-213 5B 1 5.4 T9 K90941 Seamless Tube ASTM/ASME A/SA-213 15E 1 6.4 T91 K90901 Seamless Tube ASTM/ASME A/SA-213 15E 1 6.4 T92 K92460 Seamless Tube ASTM/ASME A/SA-213 8 3 8.3 TP201 S20100 Seamless Tube ASTM/ASME A/SA-213 8 3 8.3 TP202 S20200 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP304 S30400 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP304H S30409 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP304L S30403 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP304LN S30453 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP304N S30451 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP309Cb S30940 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP309H S30909 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP309HCb S30941 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP309S S30908 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP310Cb S31040 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP310H S31009 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP310HCb S31041 Seamless Tube ASTM/ASME A/SA-213 8 3 8.2 TP310HCbN S31042 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP310MoLN S31050 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP310MoLN S31050 Seamless Tube ASTM/ASME A/SA-213 8 2 8.2 TP310S S31008 Seamless Tube
(Continued)
12 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-213 8 1 8.1 TP316 S31600 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP316H S31609 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP316L S31603 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP316LN S31653 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP316N S31651 Seamless Tube ASTM A213 8 1 8.1 TP316Ti S31635 Seamless Tube ASTM A213 8 1 8.1 TP317 S31700 Seamless Tube ASTM A213 8 1 8.1 TP317L S31703 Seamless Tube ASTM/ASME A/SA-213 8 4 8.1 TP317LM S31725 Seamless Tube ASTM/ASME A/SA-213 8 4 8.1 TP317LMN S31726 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP321 S32100 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP321H S32109 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP347 S34700 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP347H S34709 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP347HFG S34710 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP347LN S34751 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP348 S34800 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 TP348H S34809 Seamless Tube ASTM/ASME A/SA-213 8 1 8.1 XM-15 S38100 Seamless Tube ASTM/ASME A/SA-213 8 3 8.3 XM-19 S20910 Seamless Tube ASTM/ASME A/SA-214 1 1 1.1 — K01807 E.R.W. Tube ASTM/ASME A/SA-216 1 1 1.1 WCA J02502 Castings ASTM/ASME A/SA-216 1 2 1.1 WCB J03002 Castings ASTM/ASME A/SA-216 1 2 1.1 WCC J02503 Castings ASTM/ASME A/SA-217 5B 1 5.4 C12 J82090 Castings ASTM A217 15E 1 6.4 C12A J84090 Castings ASTM/ASME A/SA-217 5B 1 5.3 C5 J42045 Castings ASTM/ASME A/SA-217 6 3 7.2 CA15 J91150 Castings ASTM/ASME A/SA-217 3 1 1.1 WC1 J12524 Castings ASTM/ASME A/SA-217 4 1 9.1 WC4 J12082 Castings ASTM/ASME A/SA-217 4 1 4.2 WC5 J22000 Castings ASTM/ASME A/SA-217 4 1 5.1 WC6 J12072 Castings ASTM/ASME A/SA-217 5A 1 5.2 WC9 J21890 Castings ASTM/ASME A/SA-225 10A 1 4.1 C K12524 Plate ASTM/ASME A/SA-225 10A 1 2.1 D K12004 Plate ASTM/ASME A/SA-225 10A 1 2.1 D K12004 Plate ASTM A226 1 1 1.1 — K01201 E.R.W. Tube ASTM/ASME A/SA-234 3 1 11.2 WP1 K12821 Piping Fittings ASTM/ASME A/SA-234 4 1 5.1 WP11, Cl.1 — Piping Fittings ASTM/ASME A/SA-234 4 1 5.1 WP11, Cl.2 — Piping Fittings ASTM/ASME A/SA-234 4 1 5.1 WP11, Cl.3 — Piping Fittings ASTM/ASME A/SA-234 4 1 5.1 WP12, Cl.1 K12062 Piping Fittings
(Continued)
13 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-234 4 1 5.1 WP12, Cl. 2 K12062 Piping Fittings ASTM/ASME A/SA-234 5A 1 5.2 WP22, Cl. 1 K21590 Piping Fittings ASTM/ASME A/SA-234 5A 1 5.2 WP22, Cl. 3 K21590 Piping Fittings ASTM/ASME A/SA-234 5B 1 5.3 WP5, Cl. 1 K41545 Piping Fittings ASTM/ASME A/SA-234 5B 1 5.3 WP5, Cl. 3 K41545 Piping Fittings ASTM/ASME A/SA-234 5B 1 5.4 WP9, Cl. 1 K90941 Piping Fittings ASTM/ASME A/SA-234 5B 1 5.4 WP9, Cl. 3 K90941 Piping Fittings ASTM/ASME A/SA-234 15E 1 6.4 WP91 K90901 Piping Fittings ASTM/ASME A/SA-234 1 1 11.1 WPB K03006 Piping Fittings ASTM/ASME A/SA-234 1 2 11.1 WPC K03501 Piping Fittings ASTM/ASME A/SA-234 9A 1 9.1 WPR K22035 Piping Fittings ASTM/ASME A/SA-240 8 3 8.3 — S20400 Plate, Sheet, & Strip ASTM/ASME A/SA-240 45 — 8.2 — S31277 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.1 — S32003 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 4 8.2 — S32053 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.1 — S32101 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.1 — S32101 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.1 — S32202 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 3 8.3 201-1 S20100 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 3 8.3 201-2 S20100 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 3 8.3 201LN S20153 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 3 8.3 202 S20200 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.1 2205 S32205 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 301 S30100 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 302 S30200 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 304 S30400 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 304H S30409 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 304L S30403 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 304LN S30453 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 304N S30451 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 305 S30500 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 309Cb S30940 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 309H S30909 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 309HCb S30941 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 309S S30908 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 310Cb S31040 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 310H S31009 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 310HCb S31041 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 310MoLN S31050 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 310MoLN S31050 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 310S S31008 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 316 S31600 Plate, Sheet, & Strip
(Continued)
14 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-240 8 1 8.1 316Cb S31640 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 316H S31609 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 316L S31603 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 316LN S31653 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 316N S31651 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 316Ti S31635 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 317 S31700 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 317L S31703 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 321 S32100 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 321H S32109 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.2 329 S32900 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 347 S34700 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 347H S34709 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 348 S34800 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 348H S34809 Plate, Sheet, & Strip ASTM/ASME A/SA-240 7 1 7.1 405 S40500 Plate, Sheet, & Strip ASTM/ASME A/SA-240 7 1 7.1 409 S40910 Plate, Sheet, & Strip ASTM/ASME A/SA-240 7 1 7.1 409 S40920 Plate, Sheet, & Strip ASTM/ASME A/SA-240 7 1 7.1 409 S40930 Plate, Sheet, & Strip ASTM/ASME A/SA-240 6 1 7.2 410 S41000 Plate, Sheet, & Strip ASTM/ASME A/SA-240 7 1 7.2 410S S41008 Plate, Sheet, & Strip ASTM/ASME A/SA-240 6 2 7.2 429 S42900 Plate, Sheet, & Strip ASTM/ASME A/SA-240 7 2 7.1 430 S43000 Plate, Sheet, & Strip ASTM/ASME A/SA-240 7 2 7.1 439 S43035 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 3 8.1 S21800 S21800 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 S30600 S30600 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 S30601 S30601 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 2 8.2 S30815 S30815 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.2 S31200 S31200 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 4 8.2 S31254 S31254 Sheet & Strip ASTM/ASME A/SA-240 8 4 8.2 S31254 S31254 Plate ASTM/ASME A/SA-240 10H 1 10.2 S31260 S31260 Plate, Sheet, & Strip ASTM/ASME A/SA-240 45 — 8.2 S31277 S31277 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 4 8.1 S31725 S31725 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 4 8.1 S31726 S31726 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 S31753 S31753 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.1 S31803 S31803 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.2 S32550 S32550 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 S32615 S32615 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.2 S32750 S32750 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.2 S32760 S32760 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.2 S32906 S32906 Plate, Sheet, & Strip
(Continued)
15 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-240 10H 1 10.2 S32906 S32906 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10H 1 10.2 S32950 S32950 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 4 8.3 S34565 S34565 Plate, Sheet, & Strip ASTM/ASME A/SA-240 6 4 7.2 S41500 S41500 Plate, Sheet, & Strip ASTM/ASME A/SA-240 7 2 7.1 S43932 S43932 Plate, Sheet, & Strip ASTM/ASME A/SA-240 7 2 7.1 S44400 S44400 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10I 1 7.1 S44635 S44635 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10K 1 7.1 S44660 S44660 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10J 1 7.1 S44700 S44700 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10K 1 7.1 S44800 S44800 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 1 8.1 XM-15 S38100 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 3 8.3 XM-17 S21600 Plate ASTM/ASME A/SA-240 8 3 8.3 XM-17 S21600 Sheet & Strip ASTM/ASME A/SA-240 8 3 8.3 XM-18 S21603 Plate ASTM/ASME A/SA-240 8 3 8.3 XM-18 S21603 Sheet & Strip ASTM/ASME A/SA-240 8 3 8.3 XM-19 S20910 Sheet & Strip ASTM/ASME A/SA-240 8 3 8.3 XM-19 S20910 Plate ASTM/ASME A/SA-240 8 1 8.1 XM-21 S30452 Plate ASTM/ASME A/SA-240 8 1 8.1 XM-21 S30452 Sheet & Strip ASTM/ASME A/SA-240 10I 1 7.1 XM-27 S44627 Plate, Sheet, & Strip ASTM/ASME A/SA-240 8 3 8.3 XM-29 S24000 Plate, Sheet, & Strip ASTM/ASME A/SA-240 10I 1 7.1 XM-33 S44626 Plate, Sheet, & Strip ASTM A242 1 2 1.2 1 K11510 Plate, Bar, & Shapes ASTM A242 1 2 1.2 1 K11510 Plate, Bar, & Shapes ASTM A242 1 2 1.2 1 K11510 Plate, Bar, & Shapes ASTM/ASME A/SA-249 8 4 8.2 — S32053 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 S30815 S30815 Welded Tube ASTM/ASME A/SA-249 8 4 8.2 S31254 S31254 Welded Tube ASTM/ASME A/SA-249 8 4 8.2 S31254 S31254 Welded Tube ASTM/ASME A/SA-249 8 4 8.1 S31725 S31725 Welded Tube ASTM/ASME A/SA-249 8 4 8.1 S31726 S31726 Welded Tube ASTM/ASME A/SA-249 8 3 8.3 TP 201 S20100 Welded Tube ASTM/ASME A/SA-249 8 3 8.3 TP 202 S20200 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP XM-15 S38100 Welded Tube ASTM/ASME A/SA-249 8 3 8.3 TP XM-19 S20910 Welded Tube ASTM/ASME A/SA-249 8 3 8.3 TP XM-29 S24000 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP304 S30400 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP304H S30409 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP304L S30403 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP304LN S30453 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP304N S30451 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP309 S30900 Welded Tube
(Continued)
16 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-249 8 2 8.2 TP309Cb S30940 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP309H S30909 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP309HCb S30941 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP309S S30908 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP310Cb S31040 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP310H S31009 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP310HCb S31041 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP310MoLN S31050 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP310MoLN S31050 Welded Tube ASTM/ASME A/SA-249 8 2 8.2 TP310S S31008 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP316 S31600 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP316H S31609 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP316L S31603 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP316LN S31653 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP316N S31651 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP317 S31700 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP317L S31703 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP321 S32100 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP321H S32109 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP347 S34700 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP347H S34709 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP348 S34800 Welded Tube ASTM/ASME A/SA-249 8 1 8.1 TP348H S34809 Welded Tube ASTM/ASME A/SA-250 3 1 1.1 T1 K11522 E.R.W. Tube ASTM/ASME A/SA-250 4 1 5.1 T11 K11597 E.R.W. Tube ASTM/ASME A/SA-250 4 1 5.1 T12 K11562 E.R.W. Tube ASTM/ASME A/SA-250 3 1 1.1 T1a K12023 E.R.W. Tube ASTM/ASME A/SA-250 3 1 1.1 T1b K11422 E.R.W. Tube ASTM/ASME A/SA-250 3 1 4.2 T2 K11547 E.R.W. Tube ASTM/ASME A/SA-250 5A 1 5.2 T22 K21590 E.R.W. Tube ASTM A252 1 1 — 1 — Pipe Piles ASTM A252 1 1 — 2 — Pipe Piles ASTM A252 1 1 — 3 — Pipe Piles ASTM/ASME A/SA-266 1 1 11.1 1 K03506 Forgings ASTM/ASME A/SA-266 1 2 11.1 2 K03506 Forgings ASTM/ASME A/SA-266 1 2 11.2 3 K05001 Forgings ASTM/ASME A/SA-266 1 2 11.1 4 K03017 Forgings ASTM/ASME A/SA-268 7 2 7.1 18Cr-2Mo S44400 Seamless & Welded Tube ASTM/ASME A/SA-268 10I 1 7.1 25-4-4 S44635 Seamless & Welded Tube ASTM/ASME A/SA-268 10K 1 7.1 26-3-3 S44660 Seamless & Welded Tube ASTM/ASME A/SA-268 10J 1 7.1 29-4 S44700 Seamless & Welded Tube ASTM/ASME A/SA-268 10K 1 7.1 29-4-2 S44800 Seamless & Welded Tube
(Continued)
17 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-268 7 1 7.1 S40800 S40800 Seamless & Welded Tube ASTM/ASME A/SA-268 6 4 7.2 S41500 S41500 Seamless & Welded Tube ASTM/ASME A/SA-268 10J 1 7.1 S44735 S44735 Seamless & Welded Tube ASTM/ASME A/SA-268 10I 1 7.1 TP 446-1 S44600 Seamless & Welded Tube ASTM/ASME A/SA-268 10I 1 7.1 TP 446-2 S44600 Seamless & Welded Tube ASTM/ASME A/SA-268 10I 1 7.1 TP XM-27 S44627 Seamless & Welded Tube ASTM/ASME A/SA-268 10I 1 7.1 TP XM-33 S44626 Seamless & Welded Tube ASTM/ASME A/SA-268 7 1 7.1 TP405 S40500 Seamless & Welded Tube ASTM/ASME A/SA-268 7 1 7.1 TP409 S40900 Seamless & Welded Tube ASTM/ASME A/SA-268 6 1 7.2 TP410 S41000 Seamless & Welded Tube ASTM/ASME A/SA-268 6 2 7.2 TP429 S42900 Seamless & Welded Tube ASTM/ASME A/SA-268 7 2 7.1 TP430 S43000 Seamless & Welded Tube ASTM/ASME A/SA-268 7 2 7.1 TP430Ti S43036 Seamless & Welded Tube ASTM/ASME A/SA-268 7 2 7.1 TP439 S43035 Seamless & Welded Tube ASTM A269 8 1 8.1 TP304 S30400 Seamless & Welded Tube ASTM A269 8 1 8.1 TP304L S30403 Seamless & Welded Tube ASTM A269 8 1 8.1 TP304LN S30453 Seamless & Welded Tube ASTM A269 8 1 8.1 TP316 S31600 Seamless & Welded Tube ASTM A269 8 1 8.1 TP316L S31603 Seamless & Welded Tube ASTM A269 8 1 8.1 TP316LN S31653 Seamless & Welded Tube ASTM A269 8 1 8.1 TP317 S31700 Seamless & Welded Tube ASTM A269 8 1 8.1 TP321 S32100 Seamless & Welded Tube ASTM A269 8 1 8.1 TP347 S34700 Seamless & Welded Tube ASTM A269 8 1 8.1 TP348 S34800 Seamless & Welded Tube ASTM A269 8 3 8.3 TPXM-10 S21900 Seamless & Welded Tube ASTM A269 8 3 8.3 TPXM-11 S21904 Seamless & Welded Tube ASTM A269 8 3 8.3 TPXM-15 S38100 Seamless & Welded Tube ASTM A269 8 3 8.3 TPXM-19 S20910 Seamless & Welded Tube ASTM A269 8 3 8.3 TPXM-29 S24000 Seamless & Welded Tube ASTM A270 8 1 8.1 TP304 S30400 Seamless & Welded Tube ASTM A271 8 1 8.1 TP304 S30400 Seamless Tube ASTM A271 8 1 8.1 TP304H S30409 Seamless Tube ASTM A271 8 1 8.1 TP316 S31600 Seamless Tube ASTM A271 8 1 8.1 TP316H S31609 Seamless Tube ASTM A271 8 1 8.1 TP321 S32100 Seamless Tube ASTM A271 8 1 8.1 TP321H S32109 Seamless Tube ASTM A271 8 1 8.1 TP347 S34700 Seamless Tube ASTM A271 8 1 8.1 TP347H S34709 Seamless Tube ASTM A276 10H 1 10.1 — S32101 Bar ASTM/ASME A/SA-276 10H 1 10.1 — S32550 Bars & Shapes ASTM/ASME A/SA-276 10H 1 10.1 S32205 S32205 Bar ASTM/ASME A/SA-276 8 1 8.1 TP304 S30400 Bar
(Continued)
18 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-276 8 1 8.1 TP304L S30403 Bar ASTM/ASME A/SA-276 8 1 8.1 TP316 S31600 Bar ASTM/ASME A/SA-276 8 1 8.1 TP316L S31603 Bar ASTM/ASME A/SA-276 6 1 7.2 TP410 S41000 Bar ASTM/ASME A/SA-283 1 1 1.1 A K01400 Plate ASTM/ASME A/SA-283 1 1 1.1 B K01702 Plate ASTM/ASME A/SA-283 1 1 1.1 C K02401 Plate ASTM/ASME A/SA-283 1 1 1.1 D K02702 Plate ASTM/ASME A/SA-285 1 1 1.1 A K01700 Plate ASTM/ASME A/SA-285 1 1 1.1 B K02200 Plate ASTM/ASME A/SA-285 1 1 11.1 C K02801 Plate ASTM A297 8 2 8.2 HE J93403 Castings ASTM A297 8 2 8.2 HF J92603 Castings ASTM A297 8 2 8.2 HH J93503 Castings ASTM A297 8 2 8.2 HI J94003 Castings ASTM A297 8 2 8.2 HK J94224 Castings ASTM/ASME A/SA-299 1 2 11.1 A K02803 Plate ASTM/ASME A/SA-299 1 3 11.1 B K02803 Plate ASTM/ASME A/SA-312 8 4 8.2 — S32053 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 S30600 S30600 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 S30815 S30815 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 4 8.2 S31254 S31254 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 4 8.2 S31254 S31254 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 4 8.1 S31725 S31725 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 4 8.1 S31726 S31726 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 S32615 S32615 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 4 8.3 S34565 S34565 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 3 8.3 TP XM-11 S21904 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP XM-15 S38100 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 3 8.3 TP XM-19 S20910 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 3 8.3 TP XM-29 S24000 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP304 S30400 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP304H S30409 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP304L S30403 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP304LN S30453 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP304N S30451 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 TP309Cb S30940 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 TP309H S30909 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 TP309HCb S30941 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 TP309S S30908 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 TP310Cb S31040 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 TP310H S31009 Seamless & Welded Pipe
(Continued)
19 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-312 8 2 8.2 TP310HCb S31041 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 TP310MoLN S31050 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 TP310MoLN S31050 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 2 8.2 TP310S S31008 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP316 S31600 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP316H S31609 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP316L S31603 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP316LN S31653 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP316N S31651 Seamless & Welded Pipe ASTM A312 8 1 8.1 TP316Ti S31635 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP317 S31700 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP317L S31703 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP321 S32100 Seamless Pipe ASTM/ASME A/SA-312 8 1 8.1 TP321 S32100 Seamless Pipe ASTM/ASME A/SA-312 8 1 8.1 TP321H S32109 Seamless Pipe ASTM/ASME A/SA-312 8 1 8.1 TP321H S32109 Seamless Pipe ASTM/ASME A/SA-312 8 1 8.1 TP347 S34700 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP347H S34709 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP347LN S34751 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP348 S34800 Seamless & Welded Pipe ASTM/ASME A/SA-312 8 1 8.1 TP348H S34809 Seamless & Welded Pipe ASTM/ASME A/SA-333 1 1 11.1 1 K03008 Seamless & Welded Pipe ASTM/ASME A/SA-333 1 3 11.1 10 — Seamless & Welded Pipe ASTM/ASME A/SA-333 9B 1 9.2 3 K31918 Seamless & Welded Pipe ASTM/ASME A/SA-333 4 2 4.1 4 K11267 Seamless & Welded Pipe ASTM/ASME A/SA-333 1 1 11.1 6 K03006 Seamless & Welded Pipe ASTM/ASME A/SA-333 9A 1 9.1 7 K21903 Seamless & Welded Pipe ASTM/ASME A/SA-333 11A 1 9.3 8 K81340 Seamless & Welded Pipe ASTM/ASME A/SA-333 9A 1 9.1 9 K22035 Seamless & Welded Pipe ASTM/ASME A/SA-334 1 1 11.1 1 K03008 Welded Tube ASTM/ASME A/SA-334 9B 1 9.2 3 K31918 Welded Tube ASTM/ASME A/SA-334 1 1 11.1 6 K03006 Welded Tube ASTM/ASME A/SA-334 9A 1 9.1 7 K21903 Welded Tube ASTM/ASME A/SA-334 11A 1 9.3 8 K81340 Welded Tube ASTM/ASME A/SA-334 9A 1 9.1 9 K22035 Welded Tube ASTM/ASME A/SA-335 3 1 1.1 P1 K11522 Seamless Pipe ASTM/ASME A/SA-335 4 1 5.1 P11 K11597 Seamless Pipe ASTM/ASME A/SA-335 4 1 5.1 P12 K11562 Seamless Pipe ASTM/ASME A/SA-335 3 1 — P15 K11578 Seamless Pipe ASTM/ASME A/SA-335 3 1 4.2 P2 K11547 Seamless Pipe ASTM/ASME A/SA-335 5A 1 5.2 P21 K31545 Seamless Pipe ASTM/ASME A/SA-335 5A 1 5.2 P22 K21590 Seamless Pipe
(Continued)
20 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-335 5B 1 5.3 P5 K41545 Seamless Pipe ASTM/ASME A/SA-335 5B 1 5.3 P5b K51545 Seamless Pipe ASTM/ASME A/SA-335 5B 1 5.3 P5c K41245 Seamless Pipe ASTM/ASME A/SA-335 5B 1 5.4 P9 K90941 Seamless Pipe ASTM/ASME A/SA-335 15E 1 6.4 P91 K90901 Seamless Pipe ASTM/ASME A/SA-335 15E 1 6.4 P92 K92460 Seamless Pipe ASTM/ASME A/SA-336 3 2 1.1 F1 K12520 Forgings ASTM/ASME A/SA-336 4 1 5.1 F11, Cl. 1 K11597 Forgings ASTM/ASME A/SA-336 4 1 5.1 F11, Cl. 2 K11572 Forgings ASTM/ASME A/SA-336 4 1 5.1 F11, Cl. 3 K11572 Forgings ASTM/ASME A/SA-336 4 1 5.1 F12 K11564 Forgings ASTM/ASME A/SA-336 5A 1 5.2 F21, Cl. 1 K31545 Forgings ASTM/ASME A/SA-336 5A 1 5.2 F21, Cl. 3 K31545 Forgings ASTM/ASME A/SA-336 5A 1 5.2 F22, Cl. 1 K21590 Forgings ASTM/ASME A/SA-336 5A 1 5.2 F22, Cl. 3 K21590 Forgings ASTM/ASME A/SA-336 5C 1 6.2 F22V K31835 Forgings ASTM/ASME A/SA-336 8 1 8.1 F304 S30400 Forgings ASTM/ASME A/SA-336 8 1 8.1 F304H S30409 Forgings ASTM/ASME A/SA-336 8 1 8.1 F304L S30403 Forgings ASTM/ASME A/SA-336 8 1 8.1 F304LN S30453 Forgings ASTM/ASME A/SA-336 8 1 8.1 F304N S30451 Forgings ASTM/ASME A/SA-336 8 2 8.2 F310 S31000 Forgings ASTM/ASME A/SA-336 8 1 8.1 F316 S31600 Forgings ASTM/ASME A/SA-336 8 1 8.1 F316H S31609 Forgings ASTM/ASME A/SA-336 8 1 8.1 F316L S31603 Forgings ASTM/ASME A/SA-336 8 1 8.1 F316LN S31653 Forgings ASTM/ASME A/SA-336 8 1 8.1 F316N S31651 Forgings ASTM/ASME A/SA-336 8 1 8.1 F321 S32100 Forgings ASTM/ASME A/SA-336 8 1 8.1 F321H S32109 Forgings ASTM/ASME A/SA-336 8 1 8.1 F347 S34700 Forgings ASTM/ASME A/SA-336 8 1 8.1 F347H S34709 Forgings ASTM/ASME A/SA-336 8 1 8.1 F348 S34800 Forgings ASTM/ASME A/SA-336 8 1 8.1 F348H S34809 Forgings ASTM/ASME A/SA-336 5C 1 6.2 F3V K31830 Forgings ASTM/ASME A/SA-336 5C 1 6.2 F3VCb K31390 Forgings ASTM/ASME A/SA-336 8 1 8.1 F46 S30600 Forgings ASTM/ASME A/SA-336 5B 1 5.3 F5 K41545 Forgings ASTM/ASME A/SA-336 5B 1 5.3 F5A K42544 Forgings ASTM/ASME A/SA-336 6 3 7.2 F6 S41000 Forgings ASTM/ASME A/SA-336 5B 1 5.4 F9 K90941 Forgings ASTM/ASME A/SA-336 15E 1 6.4 F91 K90901 Forgings ASTM/ASME A/SA-336 8 3 8.3 FXM-11 S21904 Forgings
(Continued)
21 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-336 8 3 8.3 FXM-19 S20910 Forgings ASTM/ASME A/SA-336 10I 1 7.1 FXM-27Cb S44627 Forgings ASTM/ASME A/SA-350 1 1 11.1 LF1 K03009 Forgings ASTM/ASME A/SA-350 1 2 11.1 LF2 K03011 Forgings ASTM/ASME A/SA-350 9B 1 9.2 LF3 K32025 Forgings ASTM/ASME A/SA-350 9A 1 9.1 LF5, Cl. 1 K13050 Forgings ASTM/ASME A/SA-350 9A 1 9.1 LF5, Cl. 2 K13050 Forgings ASTM/ASME A/SA-350 1 1 1.2 LF6, Cl. 1 K12202 Forgings ASTM/ASME A/SA-350 1 3 4.1 LF6, Cl. 2 K12202 Forgings ASTM/ASME A/SA-350 1 2 1.3 LF6, Cl. 3 K12202 Forgings ASTM/ASME A/SA-350 1 2 3.3 LF787, Cl. 2 K20747 Forgings ASTM/ASME A/SA-350 1 3 3.3 LF787, Cl. 3 K20747 Forgings ASTM/ASME A/SA-350 9A 1 9.1 LF9 K22036 Forgings ASTM A351 6 3 7.2 CA15 J91150 Castings ASTM/ASME A/SA-351 10H 1 10.2 CD3MWCuN J93380 Castings ASTM/ASME A/SA-351 10H 1 10.2 CD4MCu J93370 Castings ASTM/ASME A/SA-351 8 2 8.2 CE20N J92802 Castings ASTM/ASME A/SA-351 10H 1 10.2 CE8MN J93345 Castings ASTM/ASME A/SA-351 8 1 8.1 CF10 J92590 Castings ASTM/ASME A/SA-351 8 1 8.1 CF10M J92901 Castings ASTM/ASME A/SA-351 8 1 8.1 CF10MC J92971 Castings ASTM/ASME A/SA-351 8 1 8.1 CF3 J92500 Castings ASTM/ASME A/SA-351 8 1 8.1 CF3A J92500 Castings ASTM/ASME A/SA-351 8 1 8.1 CF3M J92800 Castings ASTM/ASME A/SA-351 8 1 8.1 CF8 J92600 Castings ASTM/ASME A/SA-351 8 1 8.1 CF8A J92600 Castings ASTM/ASME A/SA-351 8 1 8.1 CF8C J92710 Castings ASTM/ASME A/SA-351 8 1 8.1 CF8M J92900 Castings ASTM/ASME A/SA-351 8 3 8.3 CG6MMN J93790 Castings ASTM/ASME A/SA-351 8 1 8.1 CG8M J93000 Castings ASTM/ASME A/SA-351 8 2 8.2 CH10 J93401 Castings ASTM/ASME A/SA-351 8 2 8.2 CH20 J93402 Castings ASTM/ASME A/SA-351 8 2 8.2 CH8 J93400 Castings ASTM/ASME A/SA-351 8 2 8.2 CK20 J94202 Castings ASTM/ASME A/SA-351 8 4 8.2 CK3MCuN J93254 Castings ASTM/ASME A/SA-351 45 — 8.2 CN3MN J94651 Castings ASTM/ASME A/SA-351 8 2 8.2 HK30 J94203 Castings ASTM/ASME A/SA-351 8 2 8.2 HK40 J94204 Castings ASTM/ASME A/SA-351 45 — 45 HT30 N08603 Castings ASTM/ASME A/SA-352 6 4 7.2 CA6NM J91540 Castings ASTM/ASME A/SA-352 3 1 1.1 LC1 J12522 Castings ASTM/ASME A/SA-352 9A 1 9.1 LC2 J22500 Castings
(Continued)
22 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-352 11A 5 9.2 LC2-1 J42215 Castings ASTM/ASME A/SA-352 9B 1 9.3 LC3 J31550 Castings ASTM/ASME A/SA-352 9C 1 9.3 LC4 J41500 Castings ASTM/ASME A/SA-352 1 1 11.1 LCA J02504 Castings ASTM/ASME A/SA-352 1 1 1.1 LCB J03003 Castings ASTM/ASME A/SA-352 1 2 11.1 LCC J02505 Castings ASTM/ASME A/SA-353 11A 1 9.3 — K81340 Plate ASTM A356 1 2 11.1 1 J03502 Castings ASTM A356 5A 1 5.2 10 J22090 Castings ASTM A356 15E 1 6.4 12A J84090 Castings ASTM A356 3 1 1.1 2 J12523 Castings ASTM A356 4 1 5.1 6 J12073 Castings ASTM A356 4 1 6.2 8 J11697 Castings ASTM A356 4 1 6.2 9 J21610 Castings ASTM/ASME A/SA-358 8 4 8.2 — S32053 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 304 S30400 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 304H S30409 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 304L S30403 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 304LN S30453 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 304N S30451 Fusion Welded Pipe ASTM/ASME A/SA-358 8 2 8.2 309 S30900 Fusion Welded Pipe ASTM/ASME A/SA-358 8 2 8.2 309Cb S30940 Fusion Welded Pipe ASTM/ASME A/SA-358 8 2 8.2 309S S30908 Fusion Welded Pipe ASTM/ASME A/SA-358 8 2 8.2 310 S31000 Fusion Welded Pipe ASTM/ASME A/SA-358 8 2 8.2 310Cb S31040 Fusion Welded Pipe ASTM/ASME A/SA-358 8 2 8.2 310S S31008 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 316 S31600 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 316H S31609 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 316L S31603 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 316LN S31653 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 316N S31651 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 321 S32100 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 347 S34700 Fusion Welded Pipe ASTM/ASME A/SA-358 8 1 8.1 348 S34800 Fusion Welded Pipe ASTM/ASME A/SA-358 8 2 8.2 S30815 S30815 Fusion Welded Pipe ASTM/ASME A/SA-358 8 4 8.2 S31254 S31254 Fusion Welded Tube ASTM/ASME A/SA-358 8 4 8.1 S31725 S31725 Fusion Welded Pipe ASTM/ASME A/SA-358 8 4 8.1 S31726 S31726 Fusion Welded Pipe ASTM/ASME A/SA-358 8 3 8.3 XM-19 S20910 Fusion Welded Pipe ASTM/ASME A/SA-358 8 3 8.3 XM-29 S24000 Fusion Welded Pipe ASTM A366 1 1 1.1 CS — Sheet ASTM/ASME A/SA-369 3 1 1.1 FP1 K11522 Forged Pipe
(Continued)
23 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-369 4 1 5.1 FP11 K11597 Forged Pipe ASTM/ASME A/SA-369 4 1 5.1 FP12 K11562 Forged Pipe ASTM/ASME A/SA-369 3 1 4.2 FP2 K11547 Forged Pipe ASTM/ASME A/SA-369 5A 1 5.2 FP21 K31545 Forged Pipe ASTM/ASME A/SA-369 5A 1 5.2 FP22 K21590 Forged Pipe ASTM/ASME A/SA-369 5B 1 5.3 FP5 K41545 Forged Pipe ASTM/ASME A/SA-369 5B 1 5.4 FP9 K90941 Forged Pipe ASTM/ASME A/SA-369 15E 1 6.4 FP91 K90901 Forged Pipe ASTM/ASME A/SA-369 15E 1 6.4 FP92 K92460 Forged Pipe ASTM/ASME A/SA-369 1 1 1.1 FPA K02501 Forged Pipe ASTM/ASME A/SA-369 1 1 1.1 FPB K03006 Forged Pipe ASTM/ASME A/SA-372 1 1 11.1 A K03002 Forgings ASTM/ASME A/SA-372 1 2 11.1 B K04001 Forgings ASTM/ASME A/SA-376 8 1 8.1 16-8-2H S16800 Seamless Pipe ASTM/ASME A/SA-376 8 4 8.1 S31725 S31725 Seamless Pipe ASTM/ASME A/SA-376 8 4 8.1 S31726 S31726 Seamless Pipe ASTM/ASME A/SA-376 8 4 8.3 S34565 S34565 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP304 S30400 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP304 S30400 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP304H S30409 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP304LN S30453 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP304N S30451 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP316 S31600 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP316H S31609 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP316LN S31653 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP316N S31651 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP321 S32100 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP321 S32100 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP321H S32109 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP321H S32109 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP347 S34700 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP347H S34709 Seamless Pipe ASTM/ASME A/SA-376 8 1 8.1 TP348 S34800 Seamless Pipe ASTM A381 1 1 11.1 Y35 — Welded Pipe ASTM A381 1 1 11.1 Y42 — Welded Pipe ASTM A381 1 1 11.1 Y46 — Welded Pipe ASTM A381 1 1 11.1 Y48 — Welded Pipe ASTM A381 1 1 11.1 Y50 — Welded Pipe ASTM A381 1 2 11.1 Y52 — Welded Pipe ASTM A381 1 2 11.1 Y56 — Welded Pipe ASTM A381 1 2 11.1 Y60 — Welded Pipe ASTM A381 1 3 11.1 Y65 — Welded Pipe
(Continued)
24 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-387 4 1 5.1 11, Cl. 1 K11789 Plate ASTM/ASME A/SA-387 4 1 5.1 11, Cl. 2 K11789 Plate ASTM/ASME A/SA-387 4 1 5.1 12, Cl. 1 K11757 Plate ASTM/ASME A/SA-387 4 1 5.1 12, Cl. 2 K11757 Plate ASTM/ASME A/SA-387 3 1 4.2 2, Cl. 1 K12143 Plate ASTM/ASME A/SA-387 3 2 4.2 2, Cl. 2 K12143 Plate ASTM/ASME A/SA-387 5A 1 5.2 21, Cl. 1 K31545 Plate ASTM/ASME A/SA-387 5A 1 5.2 21, Cl. 2 K31545 Plate ASTM/ASME A/SA-387 5A 1 5.2 22, Cl. 1 K21590 Plate ASTM/ASME A/SA-387 5A 1 5.2 22, Cl. 2 K21590 Plate ASTM/ASME A/SA-387 5B 1 5.3 5, Cl. 1 K41545 Plate ASTM/ASME A/SA-387 5B 1 5.3 5, Cl. 2 K41545 Plate ASTM/ASME A/SA-387 5B 1 5.4 9, Cl. 1 K90941 Plate ASTM/ASME A/SA-387 5B 1 5.4 9, Cl. 2 K90941 Plate ASTM/ASME A/SA-387 15E 1 5.4 91, Cl. 2 K90901 Plate ASTM A389 4 1 6.2 C23 J12080 Castings ASTM A389 4 1 6.2 C24 J12092 Castings ASTM/ASME A/SA-403 8 4 8.2 — S31254 Wrought Piping Fittings ASTM/ASME A/SA-403 8 4 8.2 — S32053 Wrought Piping Fittings ASTM/ASME A/SA-403 8 4 8.3 S34565 S34565 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP304 S30400 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP304H S30409 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP304L S30403 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP304LN S30453 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP304N S30451 Wrought Piping Fittings ASTM/ASME A/SA-403 8 2 8.2 WP309 S30900 Wrought Piping Fittings ASTM/ASME A/SA-403 8 2 8.2 WP310 S31000 Wrought Piping Fittings ASTM/ASME A/SA-403 8 2 8.2 WP310S S31008 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP316 S31600 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP316H S31609 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP316L S31603 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP316LN S31653 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP316N S31651 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP317 S31700 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP317L S31703 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP321 S32100 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP321H S32109 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP347 S34700 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP347H S34709 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP348 S34800 Wrought Piping Fittings ASTM/ASME A/SA-403 8 1 8.1 WP348H S34809 Wrought Piping Fittings ASTM/ASME A/SA-403 8 3 8.3 WPXM-19 S20910 Wrought Piping Fittings
(Continued)
25 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A405 4 1 6.2 P24 K11591 Seamless Pipe ASTM/ASME A/SA-409 8 4 8.2 — S32053 Welded Pipe ASTM/ASME A/SA-409 8 2 8.2 S30815 S30815 Welded Pipe ASTM/ASME A/SA-409 8 4 8.2 S31254 S31254 Welded Pipe ASTM/ASME A/SA-409 8 4 8.1 S31725 S31725 Welded Pipe ASTM/ASME A/SA-409 8 4 8.1 S31726 S31726 Welded Pipe ASTM/ASME A/SA-409 8 4 8.3 S34565 S34565 Welded Pipe ASTM/ASME A/SA-409 8 1 8.1 TP304 S30400 Welded Pipe ASTM/ASME A/SA-409 8 1 8.1 TP304L S30403 Welded Pipe ASTM/ASME A/SA-409 8 2 8.2 TP309Cb S30940 Welded Pipe ASTM/ASME A/SA-409 8 2 8.2 TP309S S30908 Welded Pipe ASTM/ASME A/SA-409 8 2 8.2 TP310Cb S31040 Welded Pipe ASTM/ASME A/SA-409 8 2 8.2 TP310S S31008 Welded Pipe ASTM/ASME A/SA-409 8 1 8.1 TP316 S31600 Welded Pipe ASTM/ASME A/SA-409 8 1 8.1 TP316L S31603 Welded Pipe ASTM/ASME A/SA-409 8 1 8.1 TP317 S31700 Welded Pipe ASTM/ASME A/SA-409 8 1 8.1 TP321 S32100 Welded Pipe ASTM/ASME A/SA-409 8 1 8.1 TP347 S34700 Welded Pipe ASTM/ASME A/SA-409 8 1 8.1 TP348 S34800 Welded Pipe ASTM/ASME A/SA-414 1 1 1.1 A K01501 Sheet ASTM/ASME A/SA-414 1 1 1.1 B K02201 Sheet ASTM/ASME A/SA-414 1 1 1.1 C K02503 Sheet ASTM/ASME A/SA-414 1 1 1.1 D K02505 Sheet ASTM/ASME A/SA-414 1 1 11.1 E K02704 Sheet ASTM/ASME A/SA-414 1 2 11.1 F K03102 Sheet ASTM/ASME A/SA-414 1 2 11.1 G K03103 Sheet ASTM/ASME A/SA-420 9B 1 9.2 WPL3 K31918 Piping Fittings ASTM/ASME A/SA-420 1 1 11.1 WPL6 K03006 Piping Fittings ASTM/ASME A/SA-420 11A 1 9.3 WPL8 K81340 Piping Fittings ASTM/ASME A/SA-420 9A 1 9.1 WPL9 K22035 Piping Fittings ASTM/ASME A/SA-423 4 2 5.1 1 K11535 Seamless & Welded Tube ASTM/ASME A/SA-423 4 2 5.1 2 K11540 Seamless & Welded Tube ASTM/ASME A/SA-426 3 1 1.1 CP1 J12521 Centrifugal Cast Pipe ASTM/ASME A/SA-426 4 1 5.1 CP11 J12072 Centrifugal Cast Pipe ASTM/ASME A/SA-426 4 1 5.1 CP12 J11562 Centrifugal Cast Pipe ASTM/ASME A/SA-426 3 1 1.1 CP15 J11522 Centrifugal Cast Pipe ASTM/ASME A/SA-426 3 1 4.2 CP2 J11547 Centrifugal Cast Pipe ASTM/ASME A/SA-426 5A 1 5.2 CP21 J31545 Centrifugal Cast Pipe ASTM/ASME A/SA-426 5A 1 5.2 CP22 J21890 Centrifugal Cast Pipe ASTM/ASME A/SA-426 5B 1 5.3 CP5 J42045 Centrifugal Cast Pipe ASTM/ASME A/SA-426 5B 1 5.3 CP5b J51545 Centrifugal Cast Pipe ASTM/ASME A/SA-426 5B 1 5.4 CP9 J82090 Centrifugal Cast Pipe
(Continued)
26 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-426 6 3 7.2 CPCA15 J91150 Centrifugal Cast Pipe ASTM A430 8 1 8.1 FP16-8-2H S16800 Forged Pipe ASTM A430 8 1 8.1 FP304 S30400 Forged Pipe ASTM A430 8 1 8.1 FP304H S30409 Forged Pipe ASTM A430 8 1 8.1 FP304N S30451 Forged Pipe ASTM A430 8 1 8.1 FP316 S31600 Forged Pipe ASTM A430 8 1 8.1 FP316H S31609 Forged Pipe ASTM A430 8 1 8.1 FP316N S31651 Forged Pipe ASTM A430 8 1 8.1 FP321 S32100 Forged Pipe ASTM A430 8 1 8.1 FP321H S32109 Forged Pipe ASTM A430 8 1 8.1 FP347 S34700 Forged Pipe ASTM A430 8 1 8.1 FP347H S34709 Forged Pipe ASTM A441 1 2 — — K12211 Plate & Bar ASTM A441 1 2 — — K12211 Plate & Bar ASTM A441 1 2 — — K12211 Plate & Bar ASTM A441 1 2 — — K12211 Plate & Bar ASTM A441 1 2 — Group 1 — Shapes ASTM A441 1 2 — Group 2 — Shapes ASTM A441 1 2 — Group 3 — Shapes ASTM A441 1 2 — Group 4 — Shapes ASTM A441 1 2 — Group 5 — Shapes ASTM/ASME A/SA-451 8 2 8.2 CPE20N J92802 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 1 8.1 CPF10MC J92971 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 1 8.1 CPF3 J92500 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 1 8.1 CPF3A J92500 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 1 8.1 CPF3M J92800 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 1 8.1 CPF8 J92600 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 1 8.1 CPF8A J92600 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 1 8.1 CPF8C J92710 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 1 8.1 CPF8M J92900 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 2 8.2 CPH10 J93402 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 2 8.2 CPH20 J93402 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 2 8.2 CPH8 J93400 Centrifugal Cast Pipe ASTM/ASME A/SA-451 8 2 8.2 CPK20 J94202 Centrifugal Cast Pipe ASTM A452 8 1 8.1 TP304H S30409 Centrifugal Cast Pipe ASTM A452 8 1 8.1 TP316H S31609 Centrifugal Cast Pipe ASTM A452 8 1 8.1 TP347H S34709 Centrifugal Cast Pipe ASTM/ASME A/SA-455 1 2 11.2 — K03300 Plate ASTM/ASME A/SA-455 1 2 11.2 — K03300 Plate ASTM/ASME A/SA-455 1 2 11.2 — K03300 Plate ASTM A473 8 3 8.3 201 S20100 Forgings ASTM A473 8 3 8.3 202 S20200 Forgings
(Continued)
27 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A473 8 1 8.1 302 S30200 Forgings ASTM A473 8 1 8.1 302B S30215 Forgings ASTM A473 8 1 8.1 303 S30300 Forgings ASTM A473 8 1 8.1 303Se S30323 Forgings ASTM A473 8 1 8.1 304 S30400 Forgings ASTM A473 8 1 8.1 304 S30400 Forgings ASTM A473 8 1 8.1 304L S30403 Forgings ASTM A473 8 1 8.1 305 S30500 Forgings ASTM A473 8 2 8.2 308 S30800 Forgings ASTM A473 8 2 8.2 309 S30900 Forgings ASTM A473 8 2 8.2 309S S30908 Forgings ASTM A473 8 2 8.2 310 S31000 Forgings ASTM A473 8 2 8.2 310S S31008 Forgings ASTM A473 8 2 8.2 314 S31400 Forgings ASTM A473 8 1 8.1 316 S31600 Forgings ASTM A473 8 1 8.1 316 S31600 Forgings ASTM A473 8 1 8.1 316L S31603 Forgings ASTM A473 8 1 8.1 317 S31700 Forgings ASTM A473 8 1 8.1 321 S32100 Forgings ASTM A473 8 1 8.1 347 S34700 Forgings ASTM A473 8 1 8.1 348 S34800 Forgings ASTM A473 6 1 7.1 403 S40300 Forgings ASTM A473 7 1 7.1 405 S40500 Forgings ASTM A473 6 1 7.2 410 S41000 Forgings ASTM A473 6 4 7.2 414 S41400 Forgings ASTM A473 6 2 7.2 420 S42000 Forgings ASTM A473 6 2 7.2 429 S42900 Forgings ASTM A473 7 2 7.1 430 S43000 Forgings ASTM A473 8 2 8.2 S30815 S30815 Forgings ASTM A473 8 3 8.3 XM-10 S21900 Forgings ASTM A473 8 3 8.3 XM-11 S21904 Forgings ASTM/ASME A/SA-479 10H 1 10.1 — S31803 Bars & Shapes ASTM/ASME A/SA-479 8 4 8.2 — S32053 Bars & Shapes ASTM/ASME A/SA-479 10H 1 10.1 — S32101 Bars & Shapes ASTM/ASME A/SA-479 10H 1 10.1 — S32202 Bars & Shapes ASTM/ASME A/SA-479 10H 1 10.1 2205 S32205 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 302 S30200 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 304 S30400 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 304H S30409 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 304L S30403 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 304LN S30453 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 304N S30451 Bars & Shapes
(Continued)
28 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-479 8 2 8.2 309Cb S30940 Bars & Shapes ASTM/ASME A/SA-479 8 2 8.2 309S S30908 Bars & Shapes ASTM/ASME A/SA-479 8 2 8.2 310Cb S31040 Bars & Shapes ASTM/ASME A/SA-479 8 2 8.2 310S S31008 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 316 S31600 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 316Cb S31640 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 316H S31609 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 316L S31603 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 316LN S31653 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 316N S31651 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 316Ti S31635 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 321 S32100 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 321H S32109 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 347 S34700 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 347H S34709 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 348 S34800 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 348H S34809 Bars & Shapes ASTM/ASME A/SA-479 6 1 7.1 403 S40300 Bars & Shapes ASTM/ASME A/SA-479 7 1 7.1 405 S40500 Bars & Shapes ASTM/ASME A/SA-479 6 1 7.2 410 S41000 Bars & Shapes ASTM/ASME A/SA-479 6 4 7.2 414 S41400 Bars & Shapes ASTM/ASME A/SA-479 7 2 7.1 430 S43000 Bars & Shapes ASTM/ASME A/SA-479 7 2 7.1 439 S43035 Bars & Shapes ASTM/ASME A/SA-479 8 3 8.1 S21800 S21800 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 S30600 S30600 Bars & Shapes ASTM/ASME A/SA-479 8 2 8.2 S30815 S30815 Bars & Shapes ASTM/ASME A/SA-479 8 4 8.2 S31254 S31254 Bars & Shapes ASTM/ASME A/SA-479 8 4 8.1 S31725 S31725 Bars & Shapes ASTM/ASME A/SA-479 8 4 8.1 S31726 S31726 Bars & Shapes ASTM/ASME A/SA-479 10H 1 10.2 S32550 S32550 Bars & Shapes ASTM/ASME A/SA-479 8 1 8.1 S32615 S32615 Bars & Shapes ASTM/ASME A/SA-479 10H 1 10.2 S32750 S32750 Bars & Shapes ASTM A479 10H 1 10.2 S32906 S32906 Bars & Shapes ASTM/ASME A/SA-479 8 4 8.3 S34565 S34565 Bars & Shapes ASTM/ASME A/SA-479 6 4 7.2 S41500 S41500 Bars & Shapes ASTM/ASME A/SA-479 7 2 7.1 S44400 S44400 Bars & Shapes ASTM/ASME A/SA-479 10J 1 7.1 S44700 S44700 Bars & Shapes ASTM/ASME A/SA-479 10K 1 7.1 S44800 S44800 Bars & Shapes ASTM/ASME A/SA-479 8 3 8.3 XM-11 S21904 Bars & Shapes ASTM/ASME A/SA-479 8 3 8.3 XM-17 S21600 Bars & Shapes ASTM/ASME A/SA-479 8 3 8.3 XM-18 S21603 Bars & Shapes ASTM/ASME A/SA-479 8 3 8.3 XM-19 S20910 Bars & Shapes
(Continued)
29 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-479 10I 1 7.1 XM-27 S44627 Bars & Shapes ASTM/ASME A/SA-479 8 3 8.3 XM-29 S24000 Bars & Shapes ASTM/ASME A/SA-479 6 1 7.2 XM-30 S41040 Bars & Shapes ASTM/ASME A/SA-487 10A 1 2.1 1, Cl. A J13002 Castings ASTM/ASME A/SA-487 10A 1 2.1 1, Cl. B J13002 Castings ASTM/ASME A/SA-487 1 2 1.1 16, Cl. A J31200 Castings ASTM/ASME A/SA-487 3 3 2.1 2, Cl. A J13005 Castings ASTM/ASME A/SA-487 3 3 2.1 2, Cl. B J13005 Castings ASTM/ASME A/SA-487 3 3 3.1 4, Cl. A J13047 Castings ASTM/ASME A/SA-487 11A 3 3.1 4, Cl. B J13047 Castings ASTM/ASME A/SA-487 3 3 3.1 4, Cl. C J13047 Castings ASTM/ASME A/SA-487 11A 3 3.1 4, Cl. E J13047 Castings ASTM/ASME A/SA-487 5C 1 5.2 8, Cl. A J22091 Castings ASTM/ASME A/SA-487 5C 4 5.2 8, Cl. B J22091 Castings ASTM/ASME A/SA-487 5C 4 5.2 8, Cl. C J22091 Castings ASTM/ASME A/SA-487 6 3 7.2 CA15, Cl. B J91171 Castings ASTM/ASME A/SA-487 6 3 7.2 CA15, Cl. C J91150 Castings ASTM/ASME A/SA-487 6 3 7.2 CA15, Cl. D J91171 Castings ASTM/ASME A/SA-487 6 3 7.2 CA15M, Cl. A J91151 Castings ASTM/ASME A/SA-487 6 4 7.2 CA6NM, Cl. A J91540 Castings ASTM/ASME A/SA-487 6 4 7.2 CA6NM, Cl. B J91540 Castings ASTM A500 1 1 11.1 A K03000 Seamless & Welded Tube ASTM A500 1 1 11.1 B K03000 Seamless & Welded Tube ASTM A500 1 1 1.2 C K02705 Seamless & Welded Tube ASTM A500 1 1 11.1 D K03000 Seamless & Welded Tube ASTM A501 1 1 11.1 A K03000 Seamless & Welded Tube ASTM A501 1 1 1.2 B K03000 Seamless & Welded Tube ASTM/ASME A/SA-508 1 2 11.1 1 K13502 Forgings ASTM/ASME A/SA-508 1 2 11.1 1A K13502 Forgings ASTM/ASME A/SA-508 3 3 3.1 2, Cl. 1 K12766 Forgings ASTM/ASME A/SA-508 3 3 3.1 2, Cl. 2 K12766 Forgings ASTM/ASME A/SA-508 5C 1 5.2 22, Cl. 3 K21590 Forgings ASTM/ASME A/SA-508 3 3 3.1 3, Cl. 1 K12042 Forgings ASTM/ASME A/SA-508 3 3 3.1 3, Cl. 2 K12042 Forgings ASTM/ASME A/SA-508 5C 1 6.2 3V K31830 Forgings ASTM/ASME A/SA-508 5C 1 6.2 3VCb K31390 Forgings ASTM/ASME A/SA-508 11A 5 3.1 4N, Cl. 1 K22375 Forgings ASTM/ASME A/SA-508 11B 10 3.1 4N, Cl. 2 K22375 Forgings ASTM/ASME A/SA-508 3 3 3.1 4N, Cl. 3 K22375 Forgings ASTM/ASME A/SA-508 11A 5 3.1 5, Cl. 1 K42365 Forgings ASTM/ASME A/SA-508 11B 10 3.1 5, Cl. 2 K42365 Forgings ASTM A511 8 1 8.1 MT 302 S30200 Seamless Tube
(Continued)
30 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A511 8 1 8.1 MT 304 S30400 Seamless Tube ASTM A511 8 1 8.1 MT 304L S30403 Seamless Tube ASTM A511 8 2 8.2 MT 309S S30908 Seamless Tube ASTM A511 8 2 8.2 MT 310S S31008 Seamless Tube ASTM A511 8 1 8.1 MT 316 S31600 Seamless Tube ASTM A511 8 1 8.1 MT 316L S31603 Seamless Tube ASTM A511 8 1 8.1 MT 317 S31700 Seamless Tube ASTM A511 8 1 8.1 MT 321 S32100 Seamless Tube ASTM A511 8 1 8.1 MT 347 S34700 Seamless Tube ASTM A512 1 1 1.1 1008 G10080 Tube ASTM A512 1 1 1.1 1010 G10100 Tube ASTM A512 1 1 1.1 1012 G10120 Tube ASTM A512 1 1 1.1 1015 G10150 Tube ASTM A512 1 1 — 1016 G10160 Tube ASTM A512 1 1 1.1 1018 G10180 Tube ASTM A512 1 1 — 1019 G10190 Tube ASTM A512 1 1 1.1 1020 G10200 Tube ASTM A512 1 1 — 1021 G10210 Tube ASTM A512 1 2 11.1 1025 G10250 Tube ASTM A512 1 1 11.1 1026 G10260 Tube ASTM A512 1 2 11.1 1030 G10300 Tube ASTM A512 1 1 — 1110 G11100 Tube ASTM A512 1 1 — 1115 G11150 Tube ASTM A512 1 1 — 1117 G11170 Tube ASTM A512 1 1 1.1 MT 1010 G10100 Tube ASTM A512 1 1 1.1 MT 1015 G10150 Tube ASTM A512 1 1 1.1 MT 1020 G10200 Tube ASTM A512 1 1 1.1 MTX 1015 — Tube ASTM A512 1 1 1.1 MTX 1020 — Tube ASTM/ASME A/SA-513 1 1 1.1 1008 G10080 Tube ASTM/ASME A/SA-513 1 1 1.1 1010 G10100 Tube ASTM/ASME A/SA-513 1 1 1.1 1015 G10150 Tube ASTM A513 1 1 1.1 1015 CW G10150 Tube ASTM/ASME A/SA-513 1 1 — 1017 G10170 Tube ASTM/ASME A/SA-513 1 1 1.1 1018 G10180 Tube ASTM/ASME A/SA-513 1 1 — 1019 G10190 Tube ASTM/ASME A/SA-513 1 1 1.1 1020 G10200 Tube ASTM A513 1 2 1.1 1020 CW G10200 Tube ASTM/ASME A/SA-513 1 1 1.1 1021 G10210 Tube ASTM/ASME A/SA-513 1 1 1.1 1022 G10220 Tube ASTM/ASME A/SA-513 1 1 — 1023 G10230 Tube ASTM/ASME A/SA-513 1 1 — 1024 G10240 Tube
(Continued)
31 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-513 1 2 11.1 1025 G10250 Tube ASTM A513 1 2 1.2 1025 CW G10250 Tube ASTM/ASME A/SA-513 1 1 11.1 1026 G10260 Tube ASTM A513 1 3 11.1 1026 CW G10260 Tube ASTM/ASME A/SA-513 1 2 11.1 1030 G10300 Tube ASTM/ASME A/SA-513 1 1 1.1 MT 1010 G10100 Tube ASTM/ASME A/SA-513 1 1 1.1 MT 1015 G10150 Tube ASTM/ASME A/SA-513 1 1 1.1 MT 1020 G10200 Tube ASTM/ASME A/SA-513 1 1 — MTX 1015 — Tube ASTM/ASME A/SA-513 1 1 — MTX 1020 — Tube ASTM A514 11B 1 3.1 A K11856 Plate ASTM A514 11B 4 3.1 B K11630 Plate ASTM A514 11B 6 3.1 C K11511 Plate ASTM A514 11B 6 3.1 C K11511 Plate ASTM A514 11B 2 3.1 E K21604 Plate ASTM A514 11B 2 3.1 E K21604 Plate ASTM A514 11B 3 3.1 F K11576 Plate ASTM A514 11B 3 3.1 H K11646 Plate ASTM A514 11B 6 3.1 J K11625 Plate ASTM A514 11B 6 3.1 J K11625 Plate ASTM A514 11B 6 3.1 K K11523 Plate ASTM A514 11B 6 3.1 K K11523 Plate ASTM A514 11B 10 3.1 M K11683 Plate ASTM A514 11B 10 3.1 M K11683 Plate ASTM A514 11B 10 3.1 M K11683 Plate ASTM A514 11B 8 3.1 P K21650 Plate ASTM A514 11B 8 3.1 P K21650 Plate ASTM A514 11B 9 3.1 Q — Plate ASTM A514 11B 9 3.1 Q — Plate ASTM A514 11B 12 3.1 R — Plate ASTM A514 11B 12 3.1 R — Plate ASTM A514 11B 6 3.1 S — Plate ASTM A514 11B 6 3.1 T — Plate ASTM A514 11B 6 3.1 T — Plate ASTM A515 1 1 1.1 55 K02001 Plate ASTM/ASME A/SA-515 1 1 11.1 60 — Plate ASTM/ASME A/SA-515 1 1 1.1 60 K02401 Plate ASTM/ASME A/SA-515 1 1 11.1 65 K02800 Plate ASTM/ASME A/SA-515 1 2 11.1 70 K03101 Plate ASTM/ASME A/SA-516 1 1 1.1 55 K01800 Plate ASTM/ASME A/SA-516 1 1 1.1 60 K02100 Plate ASTM/ASME A/SA-516 1 1 1.1 65 K02403 Plate
(Continued)
32 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-516 1 2 11.1 70 K02700 Plate ASTM/ASME A/SA-517 11B 1 3.1 A K11856 Plate ASTM/ASME A/SA-517 11B 4 3.1 B K11630 Plate ASTM A517 11B 14 3.1 C K11511 Plate ASTM/ASME A/SA-517 11B 2 3.1 E K21604 Plate ASTM/ASME A/SA-517 11B 2 3.1 E K21604 Plate ASTM/ASME A/SA-517 11B 3 3.1 F K11576 Plate ASTM/ASME A/SA-517 11B 3 3.1 H K11646 Plate ASTM A517 11B 6 3.1 J K11625 Plate ASTM A517 11B 6 3.1 K K11523 Plate ASTM A517 11B 10 3.1 M K11683 Plate ASTM/ASME A/SA-517 11B 8 3.1 P K21650 Plate ASTM/ASME A/SA-517 11B 8 3.1 P K21650 Plate ASTM/ASME A/SA-517 11B 9 3.1 Q — Plate ASTM/ASME A/SA-517 11B 9 3.1 Q — Plate ASTM/ASME A/SA-517 11B 6 3.1 S — Plate ASTM A517 11B 6 3.1 T — Plate ASTM A519 1 1 1.1 1008 G10080 Tube ASTM A519 1 1 1.1 1012 G10120 Tube ASTM A519 1 1 1.1 1015 G10150 Tube ASTM A519 1 1 — 1016 G10160 Tube ASTM A519 1 1 — 1017 G10170 Tube ASTM A519 1 1 1.1 1018 G10180 Tube ASTM A519 1 2 1.1 1018 CW G10180 Tube ASTM A519 1 1 1.1 1018 HR G10180 Tube ASTM A519 1 1 — 1019 G10190 Tube ASTM A519 1 1 1.1 1020 G10200 Tube ASTM A519 1 2 1.1 1020 CW G10200 Tube ASTM A519 1 1 1.1 1020 HR G10200 Tube ASTM A519 1 1 — 1021 G10210 Tube ASTM A519 1 1 1.1 1022 G10220 Tube ASTM A519 1 2 1.1 1022 CW G10220 Tube ASTM A519 1 1 1.1 1022 HR G10220 Tube ASTM A519 1 2 11.1 1025 G10250 Tube ASTM A519 1 2 1.2 1025 CW G10250 Tube ASTM A519 1 1 1.1 1025 HR G10250 Tube ASTM A519 1 1 — 1026 G10260 Tube ASTM A519 1 2 11.1 1026 CW G10260 Tube ASTM A519 1 1 11.1 1026 HR G10260 Tube ASTM A519 1 2 — 1030 G10300 Tube ASTM A519 11B 9 — 4130 G41300 Tube ASTM A519 11B 9 — 8630 G86300 Tube
(Continued)
33 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A519 1 1 1.1 MT 1010 G10100 Tube ASTM A519 1 1 1.1 MT 1015 G10150 Tube ASTM A519 1 1 1.1 MT 1020 G10200 Tube ASTM A519 1 1 — MTX 1015 — Tube ASTM A519 1 1 — MTX 1020 — Tube ASTM A521 1 1 — CC — Die Forging ASTM A521 1 1 — CC1 — Die Forging ASTM A521 1 2 — CE — Die Forging ASTM/ASME A/SA-522 11A 1 9.3 I K81340 Forgings ASTM/ASME A/SA-522 11A 1 9.3 II K71340 Forgings ASTM A523 1 1 1.1 A K02504 Pipe ASTM A523 1 1 11.1 B K03005 Pipe ASTM/ASME A/SA-524 1 1 1.1 I K02104 Seamless Pipe ASTM/ASME A/SA-524 1 1 1.1 II K02104 Seamless Pipe ASTM A526 1 1 — II — Galvanized Sheet ASTM A527 1 1 — II — Galvanized Sheet ASTM A529 1 1 11.1 42 K02703 Plate, Bar, & Shapes ASTM A529 1 2 11.1 50 — Plate, Bar, & Shapes ASTM A529 1 2 11.1 55 — Plate, Bar, & Shapes ASTM/ASME A/SA-533 3 3 3.1 A, Cl. 1 K12521 Plate ASTM/ASME A/SA-533 3 3 3.1 A, Cl. 2 K12521 Plate ASTM/ASME A/SA-533 11A 4 3.1 A, Cl. 3 K12521 Plate ASTM/ASME A/SA-533 3 3 3.1 B, Cl. 1 K12539 Plate ASTM/ASME A/SA-533 3 3 3.1 B, Cl. 2 K12539 Plate ASTM/ASME A/SA-533 11A 4 3.2 B, Cl. 3 K12539 Plate ASTM/ASME A/SA-533 3 3 3.1 C, Cl. 1 K12554 Plate ASTM/ASME A/SA-533 3 3 3.1 C, Cl. 2 K12554 Plate ASTM/ASME A/SA-533 11A 4 3.2 C, Cl. 3 K12554 Plate ASTM/ASME A/SA-533 3 3 3.1 D, Cl. 1 K12529 Plate ASTM/ASME A/SA-533 3 3 3.1 D, Cl. 2 K12529 Plate ASTM/ASME A/SA-533 11A 4 3.1 D, Cl. 3 K12529 Plate ASTM/ASME A/SA-533 3 3 3.1 E, Cl. 1 K12554 Plate ASTM/ASME A/SA-533 3 3 3.1 E, Cl. 2 K12554 Plate ASTM/ASME A/SA-537 1 2 1.2 Cl. 1 K12437 Plate ASTM/ASME A/SA-537 1 2 1.2 Cl. 1 K12437 Plate ASTM/ASME A/SA-537 1 3 1.2 Cl. 2 K12437 Plate ASTM/ASME A/SA-537 1 3 1.2 Cl. 2 K12437 Plate ASTM/ASME A/SA-537 1 3 1.2 Cl. 2 K12437 Plate ASTM/ASME A/SA-537 1 3 1.2 Cl. 3 K12437 Plate ASTM/ASME A/SA-537 1 3 1.2 Cl. 3 K12437 Plate ASTM/ASME A/SA-537 1 3 1.2 Cl. 3 K12437 Plate ASTM A539 1 1 — — K01506 Coiled Tube
(Continued)
34 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-541 1 2 11.1 1 K03506 Forgings ASTM/ASME A/SA-541 4 1 5.2 11, Cl. 4 K11572 Forgings ASTM/ASME A/SA-541 1 2 11.1 1A K03020 Forgings ASTM/ASME A/SA-541 3 3 4.2 2, Cl.1 K12765 Forgings ASTM/ASME A/SA-541 3 3 4.2 2, Cl.2 K12765 Forgings ASTM/ASME A/SA-541 5C 1 5.2 22, Cl. 3 K21390 Forgings ASTM/ASME A/SA-541 5C 4 5.2 22, Cl. 4 K21390 Forgings ASTM/ASME A/SA-541 5C 5 5.2 22, Cl. 5 K21390 Forgings ASTM/ASME A/SA-541 5C 1 5.2 22V K31835 Forgings ASTM/ASME A/SA-541 3 3 4.1 3, Cl. 1 K12045 Forgings ASTM/ASME A/SA-541 3 3 4.1 3, Cl. 2 K12045 Forgings ASTM/ASME A/SA-541 5C 1 6.2 3V K31830 Forgings ASTM/ASME A/SA-541 5C 1 6.2 3VCb K31390 Forgings ASTM/ASME A/SA-542 5C 4 5.2 A, Cl. 1 K21590 Plate ASTM/ASME A/SA-542 5C 5 5.2 A, Cl. 2 K21590 Plate ASTM/ASME A/SA-542 5C 3 5.2 A, Cl. 3 K21590 Plate ASTM/ASME A/SA-542 5C 1 5.2 A, Cl. 4 K21590 Plate ASTM/ASME A/SA-542 5C 1 5.2 A, Cl. 4a K21590 Plate ASTM/ASME A/SA-542 5C 4 5.2 B, Cl. 1 K21590 Plate ASTM/ASME A/SA-542 5C 5 5.2 B, Cl. 2 K21590 Plate ASTM/ASME A/SA-542 5C 3 5.2 B, Cl. 3 K21590 Plate ASTM/ASME A/SA-542 5C 1 5.2 B, Cl. 4 K21590 Plate ASTM/ASME A/SA-542 5C 1 5.2 B, Cl. 4a K21590 Plate ASTM/ASME A/SA-542 5C 4 6.2 C, Cl. 1 K31830 Plate ASTM/ASME A/SA-542 5C 5 6.2 C, Cl. 2 K31830 Plate ASTM/ASME A/SA-542 5C 3 6.2 C, Cl. 3 K31830 Plate ASTM/ASME A/SA-542 5C 1 6.2 C, Cl. 4 K31830 Plate ASTM/ASME A/SA-542 5C 1 6.2 C, Cl. 4a K31830 Plate ASTM/ASME A/SA-542 5C 1 6.3 D, Cl. 4a K31835 Plate ASTM/ASME A/SA-542 5C 1 6.2 E, Cl. 4a K31390 Plate ASTM/ASME A/SA-543 11A 5 3.1 B Cl. 1 K42339 Plate ASTM/ASME A/SA-543 11B 10 3.1 B Cl. 2 K42339 Plate ASTM/ASME A/SA-543 3 3 3.1 B Cl. 3 K42339 Plate ASTM/ASME A/SA-543 11A 5 3.1 C Cl. 1 — Plate ASTM/ASME A/SA-543 11B 10 3.1 C Cl. 2 — Plate ASTM/ASME A/SA-543 3 3 3.1 C Cl. 3 — Plate ASTM/ASME A/SA-553 11A 1 9.3 I K81340 Plate ASTM/ASME A/SA-553 11A 1 9.3 II K71340 Plate ASTM A554 8 1 8.1 MT 302 S30200 Welded Tube ASTM A554 8 1 8.1 MT 304 S30400 Welded Tube ASTM A554 8 1 8.1 MT 304L S30403 Welded Tube ASTM A554 8 2 8.2 MT 309S S30908 Welded Tube
(Continued)
35 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A554 8 2 8.2 MT 309S-Cb S30940 Welded Tube ASTM A554 8 2 8.2 MT 310S S31008 Welded Tube ASTM A554 8 1 8.1 MT 316 S31600 Welded Tube ASTM A554 8 1 8.1 MT 316L S31603 Welded Tube ASTM A554 8 1 8.1 MT 317 S31700 Welded Tube ASTM A554 8 1 8.1 MT 321 S32100 Welded Tube ASTM A554 8 1 8.1 MT 347 S34700 Welded Tube ASTM/ASME A/SA-556 1 1 1.1 A2 K01807 Seamless Tube ASTM/ASME A/SA-556 1 1 11.1 B2 K02707 Seamless Tube ASTM/ASME A/SA-556 1 2 11.1 C2 K03006 Seamless Tube ASTM/ASME A/SA-557 1 1 1.1 A2 K01807 E.R.W. Tube ASTM/ASME A/SA-557 1 1 11.1 B2 K03007 E.R.W. Tube ASTM/ASME A/SA-557 1 2 11.1 C2 K03505 E.R.W. Tube ASTM/ASME A/SA-562 1 1 1.1 — K11224 Plate ASTM A569 1 1 1.1 30 K02502 Sheet & Strip ASTM A569 1 1 1.1 33 K02502 Sheet & Strip ASTM A569 1 1 1.1 36 K02502 Sheet & Strip ASTM A569 1 1 1.1 40 K02502 Sheet & Strip ASTM A569 1 1 1.2 45 K02502 Sheet & Strip ASTM A569 1 1 1.2 50 K02502 Sheet & Strip ASTM A570 1 1 1.1 30 K02502 Sheet & Strip ASTM A570 1 1 1.1 33 K02502 Sheet & Strip ASTM A570 1 1 1.1 36 K02502 Sheet & Strip ASTM A570 1 1 1.1 40 K02502 Sheet & Strip ASTM A570 1 1 1.2 45 K02502 Sheet & Strip ASTM A570 1 1 1.2 50 K02502 Sheet & Strip ASTM A570 1 1 1.3 55 K02502 Sheet & Strip ASTM/ASME A/SA-572 1 1 1.2 42 — Plate & Shapes ASTM/ASME A/SA-572 1 1 1.2 50 — Plate & Shapes ASTM A572 1 2 1.3 55 — Plate, Sheet, Bar, & Shapes ASTM/ASME A/SA-572 1 2 11.1 60 — Plate & Shapes ASTM A572 1 3 11.1 65 — Plate, Sheet, Bar, & Shapes ASTM A573 1 1 11.1 58 — Plate ASTM A573 1 1 11.1 65 — Plate ASTM A573 1 2 11.1 70 — Plate ASTM A575 1 1 1.1 M1008 — Bar ASTM A575 1 1 1.1 M1010 — Bar ASTM A575 1 1 1.1 M1012 — Bar ASTM A575 1 1 1.1 M1015 — Bar ASTM A575 1 1 1.1 M1017 — Bar ASTM A575 1 1 11.1 M1020 — Bar ASTM A575 1 1 11.1 M1023 — Bar
(Continued)
36 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A575 1 1 11.1 M1025 — Bar ASTM A576 1 1 1.1 G10080 — Bar ASTM A576 1 1 1.1 G10100 — Bar ASTM A576 1 1 1.1 G10120 — Bar ASTM A576 1 1 1.1 G10150 — Bar ASTM A576 1 1 1.1 G10160 — Bar ASTM A576 1 1 1.1 G10170 — Bar ASTM A576 1 1 1.1 G10180 — Bar ASTM A576 1 1 1.1 G10190 — Bar ASTM A576 1 1 1.1 G10200 — Bar ASTM A576 1 1 11.1 G10210 — Bar ASTM A576 1 1 11.1 G10220 — Bar ASTM A576 1 1 11.1 G10230 — Bar ASTM A576 1 1 11.1 G10250 — Bar ASTM/ASME A/SA-587 1 1 1.1 — K11500 E.R.W. Pipe ASTM/ASME A/SA-587 1 1 1.1 A2 K01807 E.R.W. Tube ASTM/ASME A/SA-587 1 1 — B2 K03007 E.R.W. Tube ASTM A588 3 1 1.4 A K11430 Shapes ASTM A588 3 1 1.4 A K11430 Plate & Bar ASTM A588 3 1 1.4 A K11430 Plate & Bar ASTM A588 3 1 1.4 A K11430 Plate & Bar ASTM A588 3 1 1.4 B K12043 Plate & Bar ASTM A588 3 1 1.4 B K12043 Plate & Bar ASTM A588 3 1 1.4 B K12043 Shapes ASTM A588 3 1 1.4 B K12043 Plate & Bar ASTM A588 3 1 1.4 C K11538 Plate & Bar ASTM A588 3 1 1.4 C K11538 Plate & Bar ASTM A588 3 1 1.4 C K11538 Shapes ASTM A588 3 1 1.4 C K11538 Plate & Bar ASTM A588 3 1 1.4 K — Shapes ASTM A588 3 1 1.4 K — Plate & Bar ASTM A588 3 1 1.4 K — Plate & Bar ASTM A588 3 1 1.4 K — Plate & Bar ASTM/ASME A/SA-592 11B 1 3.1 A K11856 Forgings ASTM/ASME A/SA-592 11B 2 3.1 E K11695 Forgings ASTM/ASME A/SA-592 11B 2 3.1 E K11695 Forgings ASTM/ASME A/SA-592 11B 3 3.1 F K11576 Forgings ASTM/ASME A/SA-592 11B 3 3.1 F K11576 Forgings ASTM A595 1 2 11.1 A K02004 Welded Tube ASTM A595 1 2 11.1 B K02005 Welded Tube ASTM A595 3 1 11.1 C K11526 Welded Tube ASTM A606 1 2 1.4 2, CR, AR — Sheet & Strip
(Continued)
37 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A606 1 2 1.4 2, HR, A — Sheet & Strip ASTM A606 1 2 1.4 2, HR, AR — Sheet & Strip ASTM A606 1 2 1.4 2, HR, N — Sheet & Strip ASTM A606 1 2 1.4 4, CR, AR — Sheet & Strip ASTM A606 1 2 1.4 4, HR, A — Sheet & Strip ASTM A606 1 2 1.4 4, HR, AR — Sheet & Strip ASTM A606 1 2 1.4 4, HR, N — Sheet & Strip ASTM A607 1 1 — 45 — Sheet & Strip ASTM A607 1 1 — 50 — Sheet & Strip ASTM A607 1 2 — 55 — Sheet & Strip ASTM A607 1 3 — 60 — Sheet & Strip ASTM A607 1 3 — 65 — Sheet & Strip ASTM A607 1 3 — 70 — Sheet & Strip ASTM A611 1 1 — A G10170 Sheet & Strip ASTM A611 1 1 — B G10170 Sheet & Strip ASTM A611 1 1 — C G10170 Sheet & Strip ASTM A611 1 1 1.1 D G10120 Sheet & Strip ASTM A611 1 3 — E G10170 Sheet & Strip ASTM/ASME A/SA-612 10C 1 1.3 — K02900 Plate ASTM/ASME A/SA-612 10C 1 1.3 — K02900 Plate ASTM A615 1A 4 — 40 — Rebar ASTM A615 1A 4 — 60 — Rebar ASTM A618 1 2 1.2 Ia — Tube ASTM A618 1 2 1.2 Ia — Tube ASTM A618 1 2 1.2 Ib — Seamless & Welded Tube ASTM A618 1 2 1.2 Ib K02601 Tube ASTM A618 1 2 1.2 Ib K02601 Tube ASTM A618 1 2 1.2 II K12609 Tube ASTM A618 1 2 1.2 II K12609 Tube ASTM A618 1 1 1.2 III K12700 Tube ASTM A620 1 1 1.1 A K00040 Sheet ASTM A620 1 1 1.1 B K00040 Sheet ASTM A633 1 1 1.1 A K01802 Plate & Shapes ASTM A633 1 2 1.1 C K12000 Plate & Shapes ASTM A633 1 1 1.1 C K12000 Plate & Shapes ASTM A633 1 1 1.1 D K12037 Plate & Shapes ASTM A633 1 2 1.1 D K12037 Plate & Shapes ASTM A633 1 3 4.1 E K12202 Plate & Shapes ASTM/ASME A/SA-645 11A 2 9.2 A K41583 Plate ASTM A653 1 1 — 33 — Galvanized Sheet ASTM A653 1 1 — 37 — Galvanized Sheet ASTM A653 1 1 — 40 — Galvanized Sheet
(Continued)
38 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A653 1 1 — 80 — Galvanized Sheet ASTM/ASME A/SA-656 1 1 1.2 50 K11804 Plate ASTM/ASME A/SA-656 1 1 1.3 60 K11804 Plate ASTM/ASME A/SA-656 1 2 1.3 70 K11804 Plate ASTM/ASME A/SA-656 1 3 1.3 80 K11804 Plate ASTM/ASME A/SA-656 1 1 1.2 T3, 50 — Plate ASTM/ASME A/SA-656 1 2 1.3 T3, 60 — Plate ASTM/ASME A/SA-656 1 3 2.2 T3, 70 — Plate ASTM/ASME A/SA-656 1 4 2.2 T3, 80 — Plate ASTM/ASME A/SA-656 1 1 1.2 T7, 50 — Plate ASTM/ASME A/SA-656 1 2 1.3 T7, 60 — Plate ASTM/ASME A/SA-656 1 3 2.2 T7, 70 — Plate ASTM/ASME A/SA-656 1 4 2.2 T7, 80 — Plate ASTM A659 1 1 1.1 1015 G10150 Sheet & Strip ASTM A659 1 1 — 1016 G10160 Sheet & Strip ASTM A659 1 1 — 1017 G10170 Sheet & Strip ASTM A659 1 1 1.1 1018 G10180 Sheet & Strip ASTM A659 1 1 1.1 1020 G10200 Sheet & Strip ASTM A659 1 1 — 1021 G10210 Sheet & Strip ASTM A659 1 1 — 1023 G10230 Sheet & Strip ASTM/ASME A/SA-660 1 1 11.1 WCA J02504 Centrifugal Cast Pipe ASTM/ASME A/SA-660 1 2 1.1 WCB J03003 Centrifugal Cast Pipe ASTM/ASME A/SA-660 1 2 11.1 WCC J02505 Centrifugal Cast Pipe ASTM/ASME A/SA-662 1 1 1.1 A K01701 Plate ASTM/ASME A/SA-662 1 1 1.1 B K02203 Plate ASTM/ASME A/SA-662 1 2 1.1 C K02007 Plate ASTM A663 1 1 — — — Bar ASTM A663 1 1 — 45 — Bars & Shapes ASTM A663 1 1 — 50 — Bars & Shapes ASTM A663 1 1 — 55 — Bars & Shapes ASTM A663 1 1 — 60 — Bars & Shapes ASTM A663 1 1 — 65 — Bars & Shapes ASTM A663 1 2 — 70 — Bars & Shapes ASTM A663 1 2 — 75 — Bars & Shapes ASTM A663 1 3 — 80 — Bars & Shapes ASTM/ASME A/SA-666 8 3 8.3 201-1 S20100 Plate, Sheet, & Strip ASTM/ASME A/SA-666 8 3 8.3 201-2 S20100 Plate, Sheet, & Strip ASTM/ASME A/SA-666 8 1 8.1 302 S30200 Plate, Sheet, & Strip ASTM/ASME A/SA-666 8 1 8.1 304 S30400 Plate, Sheet, & Strip ASTM/ASME A/SA-666 8 1 8.1 304L S30403 Plate, Sheet, & Strip ASTM/ASME A/SA-666 8 1 8.1 304LN S30453 Plate, Sheet, & Strip ASTM/ASME A/SA-666 8 1 8.1 304N S30451 Plate, Sheet, & Strip
(Continued)
39 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-666 8 1 8.1 316 S31600 Plate, Sheet, & Strip ASTM/ASME A/SA-666 8 1 8.1 316L S31603 Plate, Sheet, & Strip ASTM/ASME A/SA-666 8 1 8.1 316N S31651 Plate, Sheet, & Strip ASTM/ASME A/SA-666 8 3 8.3 XM-11 S21904 Plate, Sheet, & Strip ASTM A668 1 1 1.1 B G10200 Forgings ASTM A668 1 2 11.1 C G10250 Forgings ASTM A668 1 2 11.1 D G10300 Forgings ASTM A668 1 3 11.1 F — Forgings ASTM A668 1 3 11.1 F — Forgings ASTM A668 1 3 11.1 F — Forgings ASTM/ASME A/SA-671 1 1 11.1 CA55 K02801 Fusion Welded Pipe ASTM/ASME A/SA-671 1 1 1.1 CB60 K02401 Fusion Welded Pipe ASTM/ASME A/SA-671 1 1 11.1 CB65 K02800 Fusion Welded Pipe ASTM/ASME A/SA-671 1 2 11.1 CB70 K03101 Fusion Welded Pipe ASTM/ASME A/SA-671 1 1 1.1 CC60 K02100 Fusion Welded Pipe ASTM/ASME A/SA-671 1 1 1.1 CC65 K02403 Fusion Welded Pipe ASTM/ASME A/SA-671 1 2 11.1 CC70 K02700 Fusion Welded Pipe ASTM/ASME A/SA-671 1 2 1.2 CD70 K12437 Fusion Welded Pipe ASTM/ASME A/SA-671 1 3 1.2 CD80 K12437 Fusion Welded Pipe ASTM/ASME A/SA-671 1 1 11.1 CE55 K02202 Fusion Welded Pipe ASTM/ASME A/SA-671 1 1 11.1 CE60 K02402 Fusion Welded Pipe ASTM/ASME A/SA-671 1 2 11.1 CK75 K02803 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 1.1 A45 K01700 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 1.1 A50 K02200 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 11.1 A55 K02801 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 1.1 B55 K02001 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 1.1 B60 K02401 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 11.1 B65 K02800 Fusion Welded Pipe ASTM/ASME A/SA-672 1 2 11.1 B70 K03101 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 1.1 C55 K01800 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 1.1 C60 K02100 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 1.1 C65 K02403 Fusion Welded Pipe ASTM/ASME A/SA-672 1 2 11.1 C70 K02700 Fusion Welded Pipe ASTM/ASME A/SA-672 1 2 1.2 D70 K12437 Fusion Welded Pipe ASTM/ASME A/SA-672 1 3 1.2 D80 K12437 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 11.1 E55 K02202 Fusion Welded Pipe ASTM/ASME A/SA-672 1 1 11.1 E60 K02402 Fusion Welded Pipe ASTM/ASME A/SA-672 3 2 1.1 H75 K12021 Fusion Welded Pipe ASTM/ASME A/SA-672 3 3 1.2 H80 K12022 Fusion Welded Pipe ASTM/ASME A/SA-672 11A 4 3.2 J100 K12521 Fusion Welded Pipe ASTM/ASME A/SA-672 3 3 3.1 J80 — Fusion Welded Pipe ASTM/ASME A/SA-672 3 3 3.1 J90 — Fusion Welded Pipe
(Continued)
40 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-672 3 1 1.1 L65 K11820 Fusion Welded Pipe ASTM/ASME A/SA-672 3 2 1.2 L70 K12020 Fusion Welded Pipe ASTM/ASME A/SA-672 3 2 1.2 L75 K12320 Fusion Welded Pipe ASTM/ASME A/SA-672 1 2 11.1 N75 K02803 Fusion Welded Pipe ASTM/ASME A/SA-675 1 1 11.1 45 — Bar ASTM/ASME A/SA-675 1 1 11.1 50 — Bar ASTM/ASME A/SA-675 1 1 11.1 55 — Bar ASTM/ASME A/SA-675 1 1 11.1 60 — Bar ASTM/ASME A/SA-675 1 1 11.1 65 — Bar ASTM/ASME A/SA-675 1 2 11.1 70 — Bar ASTM/ASME A/SA-675 1 3 — 80 — Bar ASTM/ASME A/SA-675 1 4 — 90 — Bar ASTM A678 1 2 1.2 A K01600 Plate ASTM A678 1 3 1.3 B K02002 Plate ASTM A678 1 3 1.3 C K02204 Plate ASTM A678 1 4 1.3 C K02204 Plate ASTM A678 1 4 1.3 C K02204 Plate ASTM A678 1 4 1.3 D K12202 Plate ASTM/ASME A/SA-688 8 1 8.1 TP304 S30400 Welded Tube ASTM/ASME A/SA-688 8 1 8.1 TP304L S30403 Welded Tube ASTM/ASME A/SA-688 8 1 8.1 TP304LN S30453 Welded Tube ASTM/ASME A/SA-688 8 1 8.1 TP304N S30451 Welded Tube ASTM/ASME A/SA-688 8 1 8.1 TP316 S31600 Welded Tube ASTM/ASME A/SA-688 8 1 8.1 TP316L S31603 Welded Tube ASTM/ASME A/SA-688 8 1 8.1 TP316LN S31653 Welded Tube ASTM/ASME A/SA-688 8 1 8.1 TP316N S31651 Welded Tube ASTM/ASME A/SA-688 8 3 8.3 XM-29 S24000 Welded Tube ASTM A690 1 2 1.4 — K12249 Marine Piling—Plate & Bar ASTM/ASME A/SA-691 3 1 4.2 0.5Cr, Cl. 1 K12143 Fusion Welded Pipe ASTM/ASME A/SA-691 3 2 4.2 0.5Cr, Cl. 2 K12143 Fusion Welded Pipe ASTM/ASME A/SA-691 4 1 5.1 1.25CR, Cl. 1 K11789 Fusion Welded Pipe ASTM/ASME A/SA-691 4 1 5.1 1.25CR, Cl. 2 K11789 Fusion Welded Pipe ASTM/ASME A/SA-691 4 1 5.1 1CR, Cl. 1 K11757 Fusion Welded Pipe ASTM/ASME A/SA-691 4 1 5.1 1CR, Cl. 2 K11757 Fusion Welded Pipe ASTM/ASME A/SA-691 5A 1 5.2 2.25CR, Cl. 1 K21590 Fusion Welded Pipe ASTM/ASME A/SA-691 5A 1 5.2 2.25CR, Cl. 2 K21590 Fusion Welded Pipe ASTM/ASME A/SA-691 5A 1 5.2 3CR, Cl. 1 K31545 Fusion Welded Pipe ASTM/ASME A/SA-691 5A 1 5.2 3CR, Cl. 2 K31545 Fusion Welded Pipe ASTM/ASME A/SA-691 5B 1 5.3 5CR, Cl. 1 K41545 Fusion Welded Pipe ASTM/ASME A/SA-691 5B 1 5.3 5CR, Cl. 2 K41545 Fusion Welded Pipe ASTM/ASME A/SA-691 15E 1 6.4 91 K91560 Fusion Welded Pipe ASTM/ASME A/SA-691 3 1 1.1 CM-65 K11820 Fusion Welded Pipe
(Continued)
41 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-691 3 2 1.2 CM-70 K12020 Fusion Welded Pipe ASTM/ASME A/SA-691 3 2 1.2 CM-75 K12320 Fusion Welded Pipe ASTM/ASME A/SA-691 1 2 11.1 CMS-75 K02803 Fusion Welded Pipe ASTM/ASME A/SA-691 1 2 1.2 CMSH-70 K12437 Fusion Welded Pipe ASTM/ASME A/SA-691 1 2 1.2 CMSH-70 K12437 Fusion Welded Pipe ASTM/ASME A/SA-691 1 3 1.2 CMSH-80 K12437 Fusion Welded Pipe ASTM/ASME A/SA-691 1 3 1.2 CMSH-80 K12437 Fusion Welded Pipe ASTM A694 1 1 11.1 F42 K03014 Forgings ASTM A694 1 1 11.1 F46 K03014 Forgings ASTM A694 1 1 11.1 F48 K03014 Forgings ASTM A694 1 1 11.1 F50 K03014 Forgings ASTM A694 1 1 11.1 F52 K03014 Forgings ASTM A694 1 2 11.1 F56 K03014 Forgings ASTM A694 1 2 11.1 F60 K03014 Forgings ASTM A694 1 2 11.1 F65 K03014 Forgings ASTM A694 1 3 11.1 F70 K03014 Forgings ASTM/ASME A/SA-695 1 1 11.1 B, 35 K03504 Bar ASTM/ASME A/SA-695 1 2 11.1 B, 40 K03504 Bar ASTM/ASME A/SA-696 1 1 11.1 B K03200 Bar ASTM/ASME A/SA-696 1 2 11.1 C K03200 Bar ASTM A706 1A 4 1.3 60 — Rebar ASTM A707 1 1 1.2 L1, Cl. 1 K02302 Forgings ASTM A707 1 1 1.2 L1, Cl. 2 K02302 Forgings ASTM A707 1 1 11.1 L2, Cl. 1 K03301 Forgings ASTM A707 1 1 11.1 L2, Cl. 2 K03301 Forgings ASTM A707 1 2 11.1 L2, Cl. 3 K03301 Forgings ASTM A707 1 1 1.2 L3, Cl. 1 K12510 Forgings ASTM A707 1 1 1.2 L3, Cl. 2 K12510 Forgings ASTM A707 1 2 1.3 L3, Cl. 3 K12510 Forgings ASTM A707 1 1 — L4, Cl. 1 K12089 Forgings ASTM A707 1 1 — L4, Cl. 2 K12089 Forgings ASTM A707 1 2 — L4, Cl. 3 K12089 Forgings ASTM A707 1 1 — L5, Cl. 1 K20934 Forgings ASTM A707 1 1 — L5, Cl. 2 K20934 Forgings ASTM A707 1 2 — L5, Cl. 3 K20934 Forgings ASTM A707 1 4 — L5, Cl. 4 K20934 Forgings ASTM A707 3 1 — L6, Cl. 1 K02902 Forgings ASTM A707 3 1 — L6, Cl. 2 K02902 Forgings ASTM A707 3 2 — L6, Cl. 3 K02902 Forgings ASTM A707 3 4 — L6, Cl. 4 K02902 Forgings ASTM A707 9B 1 — L7, Cl. 1 K32218 Forgings ASTM A707 9B 1 — L7, Cl. 2 K32218 Forgings
(Continued)
42 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A707 9B 1 — L8, Cl. 1 K42247 Forgings ASTM A707 9B 1 — L8, Cl. 2 K42247 Forgings ASTM A707 9B 1 — L8, Cl. 3 K42247 Forgings ASTM A707 9B 1 — L8, Cl. 4 K42247 Forgings ASTM A709 1 1 11.1 36 — Plate, Bar, & Shapes ASTM A709 1 1 1.2 50 — Plate, Bar, & Shapes ASTM A709 1 1 1.2 50S — Plate, Bar, & Shapes ASTM A709 1 2 1.4 50W, A — Plate, Bar, & Shapes ASTM A709 1 2 1.4 50W, B — Plate, Bar, & Shapes ASTM A709 1 2 1.4 HPS 50W — Plate, Bar, & Shapes ASTM A709 11B 11 1.4 HPS 70W — Plate, Bar, & Shapes ASTM A710 12C 1 3.3 A, Cl. 1 K20747 Plate ASTM A710 12A 1 3.3 A, Cl. 2 K20747 Plate ASTM A710 12A 1 3.3 A, Cl. 2 K20747 Plate ASTM A710 12B 1 3.3 A, Cl. 3 K20747 Plate ASTM A710 12B 1 3.3 A, Cl. 3 K20747 Plate ASTM A714 9A 1 9.1 V K22035 Seamless & Welded Pipe ASTM A714 9A 1 9.1 V, E K22035 Seamless & Welded Pipe ASTM/ASME A/SA-724 1 4 3.1 A K11831 Plate ASTM/ASME A/SA-724 1 4 3.1 B K12031 Plate ASTM/ASME A/SA-724 1 4 1.1 C K12037 Plate ASTM/ASME A/SA-727 1 1 11.1 — K02506 Forgings ASTM/ASME A/SA-731 7 2 7.1 18Cr-2Mo S44400 Seamless & Welded Pipe ASTM/ASME A/SA-731 6 4 7.2 S41500 S41500 Seamless & Welded Pipe ASTM/ASME A/SA-731 10K 1 7.1 S44660 S44660 Seamless & Welded Pipe ASTM/ASME A/SA-731 10J 1 7.1 S44700 S44700 Seamless & Welded Pipe ASTM/ASME A/SA-731 10K 1 7.1 S44800 S44800 Seamless & Welded Pipe ASTM/ASME A/SA-731 7 2 7.1 TP439 S43035 Seamless & Welded Pipe ASTM/ASME A/SA-731 10I 1 7.1 TPXM-27 S44627 Seamless & Welded Pipe ASTM/ASME A/SA-731 10I 1 7.1 TPXM-33 S44626 Seamless & Welded Pipe ASTM A734 11A 2 3.1 A K21205 Plate ASTM/ASME A/SA-737 1 2 11.1 B K12001 Plate ASTM/ASME A/SA-737 1 3 4.1 C K12202 Plate ASTM/ASME A/SA-738 1 2 11.1 A K12447 Plate ASTM/ASME A/SA-738 1 3 11.1 B K12007 Plate ASTM/ASME A/SA-738 1 3 11.1 C K02008 Plate ASTM/ASME A/SA-738 1 3 11.1 C K02008 Plate ASTM/ASME A/SA-738 1 3 11.1 C K02008 Plate ASTM/ASME A/SA-739 4 1 5.1 B11 K11797 Bar ASTM/ASME A/SA-739 5A 1 5.2 B22 K21390 Bar ASTM A743 6 3 7.2 CA15 J91150 Castings ASTM A743 6 3 7.2 CA15M J91151 Castings
(Continued)
43 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A743 6 4 7.2 CA40 J91153 Castings ASTM A743 6 4 7.2 CA6NM J91540 Castings ASTM A743 6 4 7.2 CB6 J91804 Castings ASTM A743 7 1 7.1 CC50 J92615 Castings ASTM A743 8 2 8.2 CE30 J93423 Castings ASTM A743 8 1 8.1 CF10SMnN J92972 Castings ASTM A743 8 1 8.2 CF16F J92701 Castings ASTM A743 8 2 8.2 CF20 J92602 Castings ASTM A743 8 1 8.1 CF3 J92500 Castings ASTM A743 8 1 8.1 CF3M J92800 Castings ASTM A743 8 1 8.2 CF3MN J92804 Castings ASTM A743 8 1 8.1 CF8 J92600 Castings ASTM A743 8 1 8.1 CF8C J92710 Castings ASTM A743 8 1 8.1 CF8M J92900 Castings ASTM A743 8 2 8.2 CG12 J93001 Castings ASTM A743 8 1 8.2 CG3M J92999 Castings ASTM A743 8 1 8.1 CG8M J93000 Castings ASTM A743 8 2 8.2 CH10 J93401 Castings ASTM A743 8 2 8.2 CH20 J93402 Castings ASTM A743 8 4 8.2 CK3MCuN J93254 Castings ASTM A743 8 2 8.2 CN3M J94652 Castings ASTM/ASME A/SA-765 1 1 11.1 I K03046 Forgings ASTM/ASME A/SA-765 1 2 11.1 II K03047 Forgings ASTM/ASME A/SA-765 9B 1 9.2 III K32026 Forgings ASTM/ASME A/SA-765 1 3 1.1 IV K02009 Forgings ASTM A774 8 1 8.1 304L S30403 Wrought Piping Fittings ASTM A774 8 1 8.1 316L S31603 Wrought Piping Fittings ASTM A774 8 1 8.1 321 S32100 Wrought Piping Fittings ASTM A774 8 1 8.1 347 S34700 Wrought Piping Fittings ASTM A774 8 1 8.1 F317L S31703 Wrought Piping Fittings ASTM A778 8 1 8.1 304L S30403 Welded Unannealed Tube ASTM A778 8 1 8.1 316L S31603 Welded Unannealed Tube ASTM A778 8 1 8.1 321 S32100 Welded Unannealed Tube ASTM A778 8 1 8.1 347 S34700 Welded Unannealed Tube ASTM A778 8 1 8.1 F317L S31703 Welded Unannealed Tube ASTM A782 11B 4 — 1 — Plate ASTM A782 11B 4 — 1 — Plate ASTM A782 11B 4 — 1 — Plate ASTM/ASME A/SA-789 10H 1 10.1 — S32003 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.1 — S32101 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.1 — S32101 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.1 — S32202 Seamless & Welded Tube
(Continued)
44 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-789 10H 1 10.2 S31200 S31200 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.2 S31260 S31260 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.1 S31500 S31500 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.1 S31803 S31803 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.1 S32205 S32205 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.1 S32304 S32304 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.1 S32304 S32304 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.2 S32550 S32550 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.2 S32750 S32750 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.2 S32760 S32760 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.2 S32900 S32900 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.2 S32906 S32906 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.2 S32906 S32906 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.2 S32950 S32950 Seamless & Welded Tube ASTM/ASME A/SA-789 10H 1 10.2 S39274 S39274 Seamless & Welded Tube ASTM/ASME A/SA-790 10H 1 10.1 — S32003 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.1 — S32101 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.1 — S32101 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.1 — S32202 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S31200 S31200 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S31260 S31260 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.1 S31500 S31500 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.1 S31803 S31803 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.1 S32205 S32205 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.1 S32304 S32304 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S32550 S32550 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S32750 S32750 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S32760 S32760 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S32900 S32900 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S32906 S32906 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S32906 S32906 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S32950 S32950 Seamless & Welded Pipe ASTM/ASME A/SA-790 10H 1 10.2 S39274 S39274 Seamless & Welded Pipe ASTM A795 1 1 — E, A — Resistance Welded Pipe ASTM A795 1 1 — E, B — Resistance Welded Pipe ASTM A795 1 1 — F — Furnace Welded Pipe ASTM A795 1 1 — S, A — Seamless Pipe ASTM A795 1 1 — S, B — Seamless Pipe ASTM/ASME A/SA-803 10K 1 7.1 26-3-3 S44660 Welded Tube ASTM/ASME A/SA-803 7 2 7.1 TP439 S43035 Welded Tube ASTM A808 1 1 1.4 — K11852 Plate ASTM/ASME A/SA-813 8 4 8.2 — S32053 Welded Pipe
(Continued)
45 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-813 8 2 8.2 S30815 S30815 Welded Pipe ASTM/ASME A/SA-813 8 4 8.2 S31254 S31254 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP304 S30400 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP304H S30409 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP304L S30403 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP304LN S30453 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP304N S30451 Welded Pipe ASTM/ASME A/SA-813 8 2 8.2 TP309Cb S30940 Welded Pipe ASTM/ASME A/SA-813 8 2 8.2 TP309S S30908 Welded Pipe ASTM/ASME A/SA-813 8 2 8.2 TP310Cb S31040 Welded Pipe ASTM/ASME A/SA-813 8 2 8.2 TP310S S31008 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP316 S31600 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP316H S31609 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP316L S31603 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP316LN S31653 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP316N S31651 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP317 S31700 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP317L S31703 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP321 S32100 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP321H S32109 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP347 S34700 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP347H S34709 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP348 S34800 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TP348H S34809 Welded Pipe ASTM/ASME A/SA-813 8 3 8.3 TPXM-11 S21904 Welded Pipe ASTM/ASME A/SA-813 8 1 8.1 TPXM-15 S38100 Welded Pipe ASTM/ASME A/SA-813 8 3 8.3 TPXM-19 S20910 Welded Pipe ASTM/ASME A/SA-813 8 3 8.3 TPXM-29 S24000 Welded Pipe ASTM/ASME A/SA-814 8 4 8.2 — S32053 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 2 8.2 S30815 S30815 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 4 8.2 S31254 S31254 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP304 S30400 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP304H S30409 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP304L S30403 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP304LN S30453 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP304N S30451 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 2 8.2 TP309Cb S30940 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 2 8.2 TP309S S30908 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 2 8.2 TP310Cb S31040 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 2 8.2 TP310S S31008 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP316 S31600 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP316H S31609 Cold Worked Welded Pipe
(Continued)
46 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-814 8 1 8.1 TP316L S31603 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP316LN S31653 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP316N S31651 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP317 S31700 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP317L S31703 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP321 S32100 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP321H S32109 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP347 S34700 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP347H S34709 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP348 S34800 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TP348H S34809 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 3 8.3 TPXM-11 S21904 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 1 8.1 TPXM-15 S38100 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 3 8.3 TPXM-19 S20910 Cold Worked Welded Pipe ASTM/ASME A/SA-814 8 3 8.3 TPXM-29 S24000 Cold Worked Welded Pipe ASTM/ASME A/SA-815 10H 1 10.1 — S32101 Fittings ASTM/ASME A/SA-815 10H 1 10.1 — S32202 Fittings ASTM/ASME A/SA-815 10H 1 10.1 S31803 S31803 Fittings ASTM/ASME A/SA-815 10H 1 10.1 S32205 S32205 Fittings ASTM/ASME A/SA-815 10H 1 10.2 S32550 S32550 Fittings ASTM/ASME A/SA-815 10H 1 10.2 S32750 S32750 Fittings ASTM/ASME A/SA-815 10H 1 10.2 S32760 S32760 Fittings ASTM/ASME A/SA-815 6 4 7.2 S41500 S41500 Fittings ASTM A830 1 1 1.1 1006 G10060 Plate ASTM A830 1 1 1.1 1008 G10080 Plate ASTM A830 1 1 1.1 1009 G10090 Plate ASTM A830 1 1 1.1 1010 G10100 Plate ASTM A830 1 1 1.1 1012 G10120 Plate ASTM A830 1 1 1.1 1015 G10150 Plate ASTM A830 1 1 1.1 1016 G10160 Plate ASTM A830 1 1 1.1 1017 G10170 Plate ASTM A830 1 1 1.1 1018 G10180 Plate ASTM A830 1 1 1.1 1019 G10190 Plate ASTM A830 1 1 1.1 1020 G10200 Plate ASTM A830 1 1 1.1 1021 G10210 Plate ASTM A830 1 1 1.1 1022 G10220 Plate ASTM A830 1 1 11.1 1023 G10230 Plate ASTM A830 1 2 11.1 1025 G10250 Plate ASTM/ASME A/SA-832 5C 1 6.2 21V K31830 Plate ASTM/ASME A/SA-832 5C 1 6.2 22V K31835 Plate ASTM/ASME A/SA-832 5C 1 6.2 23V — Plate ASTM/ASME A/SA-836 1 1 1.1 — — Forgings
(Continued)
47 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-841 1 2 1.2 A, Cl. 1 — Plate ASTM/ASME A/SA-841 1 2 1.2 A, Cl. 1 — Plate ASTM/ASME A/SA-841 1 3 1.3 B, Cl. 2 — Plate ASTM/ASME A/SA-841 1 3 1.3 B, Cl. 2 — Plate ASTM A844 11A 1 9.3 — K81340 Plate ASTM A852 11B 11 4.2 — K12043 Plate ASTM A857 1 1 1.1 25 — Sheet & Strip ASTM A857 1 1 1.1 30 — Sheet & Strip ASTM A857 1 1 1.1 33 — Sheet & Strip ASTM A857 1 1 1.1 36 — Sheet & Strip ASTM/ASME A/SA-859 11C 1 3.3 A, Cl. 1 K20747 Forgings ASTM/ASME A/SA-859 11C 1 3.3 A, Cl. 2 K20747 Forgings ASTM A871 3 2 4.2 60 — Plate ASTM A871 3 3 4.2 65 — Plate ASTM A890 10H 1 10.2 1A J93370 Castings ASTM A890 10H 1 10.2 1B J93372 Castings ASTM A890 10H 1 10.2 1C J93373 Castings ASTM A890 10H 1 10.2 2A J93345 Castings ASTM A890 10H 1 10.2 3A J93371 Castings ASTM A890 10H 1 10.1 4A J92205 Castings ASTM A890 10H 1 10.2 5A J93404 Castings ASTM A890 10H 1 10.2 6A J93380 Castings ASTM A913 1 2 1.2 50 — Shapes ASTM A913 1 3 3.1 60 — Shapes ASTM A913 1 3 3.1 65 — Shapes ASTM A913 1 3 3.1 70 — Shapes ASTM A928 10H 1 10.2 — S32760 Welded Pipe ASTM A928 10H 1 10.1 2205 S32205 Welded Pipe ASTM A928 10H 1 10.2 255 S32550 Welded Pipe ASTM A935 1 1 1.2 45, Cl. 1 — Sheet & Strip ASTM A935 1 1 1.2 45, Cl. 2 — Sheet & Strip ASTM A935 1 1 1.2 50, Cl. 1 — Sheet & Strip ASTM A935 1 1 1.2 50, Cl. 2 — Sheet & Strip ASTM A935 1 2 1.3 55, Cl. 1 — Sheet & Strip ASTM A935 1 1 1.3 55, Cl. 2 — Sheet & Strip ASTM A935 1 2 11.1 60, Cl. 1 — Sheet & Strip ASTM A935 1 2 1.3 60, Cl. 2 — Sheet & Strip ASTM A935 1 3 11.1 65, Cl. 1 — Sheet & Strip ASTM A935 1 2 1.3 65, Cl. 2 — Sheet & Strip ASTM A935 1 3 11.1 70, Cl. 1 — Sheet & Strip ASTM A935 1 3 1.3 70, Cl. 2 — Sheet & Strip ASTM/ASME A/SA-965 8 1 8.1 F304 S30400 Forgings
(Continued)
48 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM/ASME A/SA-965 8 1 8.1 F304H S30409 Forgings ASTM/ASME A/SA-965 8 1 8.1 F304L S30403 Forgings ASTM/ASME A/SA-965 8 1 8.1 F304LN S30453 Forgings ASTM/ASME A/SA-965 8 1 8.1 F304N S30451 Forgings ASTM/ASME A/SA-965 8 2 8.2 F310 S31000 Forgings ASTM/ASME A/SA-965 8 1 8.1 F316 S31600 Forgings ASTM/ASME A/SA-965 8 1 8.1 F316H S31609 Forgings ASTM/ASME A/SA-965 8 1 8.1 F316L S31603 Forgings ASTM/ASME A/SA-965 8 1 8.1 F316LN S31653 Forgings ASTM/ASME A/SA-965 8 1 8.1 F316N S31651 Forgings ASTM/ASME A/SA-965 8 1 8.1 F321 S32100 Forgings ASTM/ASME A/SA-965 8 1 8.1 F321H S32109 Forgings ASTM/ASME A/SA-965 8 1 8.1 F347 S34700 Forgings ASTM/ASME A/SA-965 8 1 8.1 F347H S34709 Forgings ASTM/ASME A/SA-965 8 1 8.1 F348 S34800 Forgings ASTM/ASME A/SA-965 8 1 8.1 F348H S34809 Forgings ASTM/ASME A/SA-965 8 1 8.1 F46 S30600 Forgings ASTM/ASME A/SA-965 8 3 8.3 FXM-11 S21904 Forgings ASTM/ASME A/SA-965 8 3 8.3 FXM-19 S20910 Forgings ASTM A984 1 1 1.1 35 — Pipe ASTM A984 1 2 1.2 50 — Pipe ASTM A984 1 2 1.3 60 — Pipe ASTM A984 1 3 — 70 — Pipe ASTM A984 1 4 — 80 — Pipe ASTM A992 1 1 1.1 — — Shapes ASTM A992 1 1 1.2 — — Plate & Shapes ASTM/ASME A/SA-995 10H 1 10.2 1B J93372 Castings ASTM/ASME A/SA-995 10H 1 10.2 2A J93345 Castings ASTM/ASME A/SA-995 10H 1 10.2 3A J93371 Castings ASTM/ASME A/SA-995 10H 1 10.1 4A J92205 Castings ASTM/ASME A/SA-995 10H 1 10.2 5A J93404 Castings ASTM/ASME A/SA-995 10H 1 10.2 6A J93380 Castings ASTM/ASME A/SA-1008 1 1 1.1 CS, A — Sheet ASTM/ASME A/SA-1008 1 1 1.1 CS, B — Sheet ASTM A1008 1 1 1.1 CS, C — Sheet ASTM A1008 1 1 1.1 DS, A — Sheet ASTM/ASME A/SA-1008 1 1 1.1 DS, B — Sheet ASTM A1008 1 1 1.2 HSLAS 45, Cl. 1 — Sheet ASTM A1008 1 1 1.2 HSLAS 45, Cl. 2 — Sheet ASTM A1008 1 1 1.2 HSLAS 50, Cl. 1 — Sheet ASTM A1008 1 1 1.2 HSLAS 50, Cl. 2 — Sheet ASTM A1008 1 2 1.3 HSLAS 55, Cl. 1 — Sheet
(Continued)
49 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A1008 1 1 1.3 HSLAS 55, Cl. 2 — Sheet ASTM A1008 1 2 11.1 HSLAS 60, Cl. 1 — Sheet ASTM A1008 1 2 1.3 HSLAS 60, Cl. 2 — Sheet ASTM A1008 1 3 11.1 HSLAS 65, Cl. 1 — Sheet ASTM A1008 1 2 1.3 HSLAS 65, Cl. 2 — Sheet ASTM A1008 1 3 11.1 HSLAS 70, Cl. 1 — Sheet ASTM A1008 1 3 1.3 HSLAS 70, Cl. 2 — Sheet ASTM A1008 1 1 1.2 HSLAS-F 50 — Sheet ASTM A1008 1 2 1.3 HSLAS-F 60 — Sheet ASTM A1008 1 3 1.3 HSLAS-F 70 — Sheet ASTM A1008 1 4 1.3 HSLAS-F 80 — Sheet ASTM A1008 1 1 1.1 SS 25 — Sheet ASTM A1008 1 1 1.1 SS 30 — Sheet ASTM A1008 1 1 1.1 SS 33, 1 — Sheet ASTM A1008 1 1 1.1 SS 33, 2 — Sheet ASTM A1008 1 1 1.1 SS 40, 1 — Sheet ASTM A1008 1 1 1.1 SS 40, 2 — Sheet ASTM A1008 1 3 1.3 SS 80 — Sheet ASTM/ASME A/SA-1010 7 1 7.2 40 S41003 Plate, Sheet, & Strip ASTM/ASME A/SA-1010 7 1 7.2 50 S41003 Plate, Sheet, & Strip ASTM A1011 1 1 1.1 CS, A — Sheet & Strip ASTM/ASME A/SA-1011 1 1 1.1 CS, B — Sheet & Strip ASTM A1011 1 1 1.1 CS, C — Sheet & Strip ASTM A1011 1 1 1.1 CS, D — Sheet & Strip ASTM A1011 1 1 1.1 DS, A — Sheet & Strip ASTM/ASME A/SA-1011 1 1 1.1 DS, B — Sheet & Strip ASTM A1011 1 1 1.2 HSLAS 45, Cl. 1 — Sheet & Strip ASTM A1011 1 1 1.2 HSLAS 45, Cl. 2 — Sheet & Strip ASTM A1011 1 1 1.2 HSLAS 50, Cl. 1 — Sheet & Strip ASTM A1011 1 1 1.2 HSLAS 50, Cl. 2 — Sheet & Strip ASTM A1011 1 2 1.3 HSLAS 55, Cl. 1 — Sheet & Strip ASTM A1011 1 1 1.3 HSLAS 5,5 Cl. 2 — Sheet & Strip ASTM A1011 1 2 11.1 HSLAS 60, Cl. 1 — Sheet & Strip ASTM A1011 1 2 1.3 HSLAS 60, Cl. 2 — Sheet & Strip ASTM A1011 1 3 11.1 HSLAS 65, Cl. 1 — Sheet & Strip ASTM A1011 1 2 1.3 HSLAS 65, Cl. 2 — Sheet & Strip ASTM A1011 1 3 11.1 HSLAS 70, Cl. 1 — Sheet & Strip ASTM A1011 1 3 1.3 HSLAS 70, Cl. 2 — Sheet & Strip ASTM A1011 1 1 1.2 HSLAS-F 50 — Sheet & Strip ASTM A1011 1 2 1.3 HSLAS-F 60 — Sheet & Strip ASTM A1011 1 3 1.3 HSLAS-F 70 — Sheet & Strip ASTM A1011 1 4 1.3 HSLAS-F 80 — Sheet & Strip
(Continued)
50 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys ASTM A1011 1 1 1.1 SS 30 — Sheet & Strip ASTM A1011 1 1 1.1 SS 33 — Sheet & Strip ASTM A1011 1 1 1.1 SS 36, 1 — Sheet & Strip ASTM A1011 1 1 1.1 SS 36, 2 — Sheet & Strip ASTM A1011 1 1 1.1 SS 40 — Sheet & Strip ASTM A1011 1 1 1.2 SS 45, 1 — Sheet & Strip ASTM A1011 1 1 1.2 SS 45, 2 — Sheet & Strip ASTM A1011 1 1 1.2 SS 50 — Sheet & Strip ASTM A1011 1 2 1.3 SS 55 — Sheet & Strip ASTM A1011 1 2 1.3 SS 60 — Sheet & Strip ASTM A1011 1 3 1.3 SS 70 — Sheet & Strip ASTM A1011 1 4 1.3 SS 80 — Sheet & Strip ASTM A1018 1 1 1.2 HSLAS 45, Cl. 1 — Sheet & Strip ASTM A1018 1 1 1.2 HSLAS 45, Cl. 2 — Sheet & Strip ASTM A1018 1 1 1.2 HSLAS 50, Cl. 1 — Sheet & Strip ASTM A1018 1 1 1.2 HSLAS 50, Cl. 2 — Sheet & Strip ASTM A1018 1 2 1.3 HSLAS 55, Cl. 1 — Sheet & Strip ASTM A1018 1 1 1.3 HSLAS 5,5 Cl. 2 — Sheet & Strip ASTM A1018 1 2 11.1 HSLAS 60, Cl. 1 — Sheet & Strip ASTM A1018 1 2 1.3 HSLAS 60, Cl. 2 — Sheet & Strip ASTM A1018 1 2 11.1 HSLAS 65, Cl. 1 — Sheet & Strip ASTM A1018 1 2 1.3 HSLAS 65, Cl. 2 — Sheet & Strip ASTM A1018 1 3 11.1 HSLAS 70, Cl. 1 — Sheet & Strip ASTM A1018 1 3 1.3 HSLAS 70, Cl. 2 — Sheet & Strip ASTM A1018 1 1 1.2 HSLAS-F 50 — Sheet & Strip ASTM A1018 1 3 1.3 HSLAS-F 60 — Sheet & Strip ASTM A1018 1 3 1.3 HSLAS-F 70 — Sheet & Strip ASTM A1018 1 4 1.3 HSLAS-F 80 — Sheet & Strip ASTM A1018 1 1 1.1 SS 30 — Sheet & Strip ASTM A1018 1 1 1.1 SS 33 — Sheet & Strip ASTM A1018 1 1 1.1 SS 36, 1 — Sheet & Strip ASTM A1018 1 1 1.1 SS 36, 2 — Sheet & Strip ASTM A1018 1 1 1.1 SS 40 — Sheet & Strip CSA G30.18 1A 4 — 300R — Rebar CSA G30.18 1A 4 — 400R — Rebar CSA G30.18 1A 4 11.1 400W — Rebar CSA G30.18 1A 4 — 500R — Rebar CSA G30.18 1A 4 11.1 500W — Rebar CSA G40.21 1 1 1.1 260W — Plate, Bar, & Shapes CSA G40.21 1 1 1.1 260WT — Plate, Bar, & Shapes CSA G40.21 1 1 1.2 300W — Plate, Bar, & Shapes CSA G40.21 1 1 1.2 300WT — Plate, Bar, & Shapes
(Continued)
51 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys CSA G40.21 1 2 1.4 350A — HSLA Plate, Bar, & Shapes CSA G40.21 1 2 1.4 350AT — HSLA Plate, Bar, & Shapes CSA G40.21 1 2 1.4 350R — HSLA Plate, Bar, & Shapes CSA G40.21 1 1 1.2 350W — Plate, Bar, & Shapes CSA G40.21 1 2 1.2 350WT — Plate, Bar, & Shapes CSA G40.21 1 2 1.3 380W — Plate, Bar, & Shapes CSA G40.21 1 2 1.3 380WT — Plate, Bar, & Shapes CSA G40.21 1 2 1.4 400A — HSLA Plate, Bar, & Shapes CSA G40.21 1 2 1.4 400AT — HSLA Plate, Bar, & Shapes CSA G40.21 1 2 1.3 400W — HSLA Plate, Bar, & Shapes CSA G40.21 1 2 1.3 400WT — HSLA Plate, Bar, & Shapes CSA G40.21 1 3 1.4 480A — HSLA Plate, Bar, & Shapes CSA G40.21 1 3 1.4 480AT — HSLA Plate, Bar, & Shapes CSA G40.21 1 3 11.1 480W — HSLA Plate, Bar, & Shapes CSA G40.21 1 3 11.1 480WT — HSLA Plate, Bar, & Shapes CSA G40.21 1 4 1.4 550A — Plate, Bar, & Shapes CSA G40.21 1 4 1.4 550AT — Plate, Bar, & Shapes CSA G40.21 1 4 1.3 550W — Plate, Bar, & Shapes CSA G40.21 1 4 1.3 550WT — Plate, Bar, & Shapes CSA Z245.1 1 1 11.1 172 — Pipe CSA Z245.1 1 1 11.1 207 — Pipe CSA Z245.1 1 1 11.1 241 — Pipe CSA Z245.1 1 1 11.1 290 — Pipe CSA Z245.1 1 2 11.1 317 — Pipe CSA Z245.1 1 2 11.1 359 — Pipe CSA Z245.1 1 2 11.1 386 — Pipe CSA Z245.1 1 3 11.1 414 — Pipe CSA Z245.1 1 3 11.1 448 — Pipe CSA Z245.1 1 3 11.1 483 — Pipe CSA Z245.1 1 4 11.1 550 — Pipe CSA Z245.11 1 1 11.1 207 — Fittings CSA Z245.11 1 1 11.1 241 — Fittings CSA Z245.11 1 1 11.1 290 — Fittings CSA Z245.11 1 2 11.1 317 — Fittings CSA Z245.11 1 2 11.1 359 — Fittings CSA Z245.11 1 2 11.1 386 — Fittings CSA Z245.11 1 3 11.1 414 — Fittings CSA Z245.11 1 3 11.1 448 — Fittings CSA Z245.11 1 3 11.1 483 — Fittings CSA Z245.11 1 4 11.1 550 — Fittings CSA Z245.12 1 1 11.1 248 — Flanges CSA Z245.12 1 1 11.1 290 — Flanges
(Continued)
52 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Ferrous Alloys
ISO Type, Grade, Base Metal Material Group 15608 or Alloy UNS Standard Specification Number Number Group Designation Number Product Form Steel and Steel Alloys CSA Z245.12 1 2 11.1 317 — Flanges CSA Z245.12 1 2 11.1 359 — Flanges CSA Z245.12 1 2 11.1 386 — Flanges CSA Z245.12 1 3 11.1 414 — Flanges CSA Z245.12 1 3 11.1 448 — Flanges CSA Z245.12 1 3 11.1 483 — Flanges MSS SP-75 1 1 11.1 WPHY-42 — Seamless & Welded Fittings MSS SP-75 1 1 11.1 WPHY-46 — Seamless & Welded Fittings MSS SP-75 1 1 11.1 WPHY-52 — Seamless & Welded Fittings MSS SP-75 1 2 11.1 WPHY-56 — Seamless & Welded Fittings MSS SP-75 1 2 11.1 WPHY-60 — Seamless & Welded Fittings MSS SP-75 1 2 11.1 WPHY-65 — Seamless & Welded Fittings MSS SP-75 1 3 11.1 WPHY-70 — Seamless & Welded Fittings
(Continued)
53 AWS B2.1/B2.1M-BMG:2014
Table C.1 List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form AMS 4914 — 53 R58153 54 Sheet AMS 4915 — 54 R54810 52 Plate AMS 4915 — 54 R54810 52 Plate AMS 4915 — 54 R54810 52 Plate AMS 4915 — 54 R54810 52 Plate AMS 4915 — 54 R54810 52 Sheet & Strip AMS 4919 — 54 R54620 52 Sheet AMS 4973 — 54 R54810 52 Forgings AMS 4973 — 54 R54810 52 Forgings AMS 4975 — 54 R54620 52 Bar AMS 4976 — 54 R54620 52 Forgings AMS 5711 — 44 N06635 43 Sheet ASTM B21 — 32 C46400 32.2 Rod & Bar ASTM B21 — 32 C46400 32.2 Rod & Bar ASTM B21 — 32 C46400 32.2 Rod & Bar ASTM B21 — 32 C46400 32.2 Shapes ASTM/ASME B/SB-26 208.0 26 A02080 25 Castings ASTM/ASME B/SB-26 222.0, O 26 A02220 — Castings ASTM/ASME B/SB-26 222.0, T61 26 A02220 — Castings ASTM/ASME B/SB-26 319.0, F 26 A03190 25 Castings ASTM/ASME B/SB-26 319.0, T5 26 A03190 25 Castings ASTM/ASME B/SB-26 319.0, T6 26 A03190 25 Castings ASTM/ASME B/SB-26 328.0, F 26 A03280 25 Castings ASTM/ASME B/SB-26 328.0, T6 26 A03280 25 Castings ASTM/ASME B/SB-26 356.0, F 26 A03560 24.2 Castings ASTM/ASME B/SB-26 356.0, T51 26 A03560 24.2 Castings ASTM/ASME B/SB-26 356.0, T6 26 A03560 24.2 Castings ASTM/ASME B/SB-26 356.0, T7 26 A03560 24.2 Castings ASTM/ASME B/SB-26 356.0, T71 26 A03560 24.2 Castings ASTM/ASME B/SB-26 443.0 26 A04430 24.1 Castings ASTM/ASME B/SB-26 512.0 26 A05120 23.1 Castings ASTM/ASME B/SB-26 514.0 26 A05140 23.1 Castings ASTM/ASME B/SB-26 535.0 26 A05350 — Castings ASTM/ASME B/SB-26 705.0, T5 26 A07050 23.2 Castings ASTM/ASME B/SB-26 710.0, T5 26 A07100 23.2 Castings ASTM/ASME B/SB-26 A356.0, T6 26 A13560 24.2 Castings ASTM/ASME B/SB-26 A356.0, T61 26 A13560 24.2 Castings ASTM/ASME B/SB-26 B443.0 26 A24430 24.1 Castings ASTM/ASME B/SB-42 — 31 C10200 31 Seamless Pipe ASTM/ASME B/SB-42 — 31 C10300 31 Seamless Pipe ASTM/ASME B/SB-42 — 31 C10800 31 Seamless Pipe ASTM/ASME B/SB-42 — 31 C12000 31 Seamless Pipe ASTM/ASME B/SB-42 — 31 C12200 31 Seamless Pipe ASTM/ASME B/SB-43 — 32 C23000 32.1 Seamless Pipe
(Continued)
54 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM B68 — 31 C10200 31 Tube ASTM B68 — 31 C10300 31 Tube ASTM B68 — 31 C10800 31 Tube ASTM B68 — 31 C12000 31 Tube ASTM B68 — 31 C12200 31 Tube ASTM/ASME B/SB-75 — 31 C10100 31 Seamless Tube ASTM/ASME B/SB-75 — 31 C10200 31 Seamless Tube ASTM/ASME B/SB-75 — 31 C10300 31 Seamless Tube ASTM/ASME B/SB-75 — 31 C10800 31 Seamless Tube ASTM/ASME B/SB-75 — 31 C12000 31 Seamless Tube ASTM/ASME B/SB-75 — 31 C12200 31 Seamless Tube ASTM/ASME B/SB-75 — 31 C14200 31 Seamless Tube ASTM B80 AZ91C, F 83 M11914 — Castings ASTM B80 AZ92A, F 83 M11920 — Castings ASTM B80 K1A 83 M18010 — Castings ASTM B88 — 31 C10200 31 Tube ASTM B88 — 31 C12000 31 Tube ASTM B88 — 31 C12200 31 Tube ASTM B90 AZ31B 81 M11311 — Plate & Sheet ASTM B90 AZ31C 81 M11312 — Sheet ASTM B90 AZ31C 81 M11312 — Plate & Sheet ASTM B90 HK31A 81 M13310 — Plate ASTM B90 HK31A 81 M13310 — Plate & Sheet ASTM B90 HK31A 81 M13310 — Plate ASTM B90 ZE10A 81 M16100 — Sheet ASTM B90 ZE10A 81 M16100 — Plate ASTM B90 ZE10A 81 M16100 — Sheet ASTM B91 AZ31B 81 M11311 — Forgings ASTM B91 AZ61A 81 M11610 — Forgings ASTM/ASME B/SB-96 — 33 C65100 37 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-96 — 33 C65400 37 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-96 — 33 C65500 37 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-98 — 33 C65100 37 Rod, Bar, & Shapes ASTM/ASME B/SB-98 — 33 C65500 37 Rod, Bar, & Shapes ASTM/ASME B/SB-98 — 33 C66100 37 Rod, Bar, & Shapes ASTM B107 AZ31B 81 M11311 — Bar, Rods, Profiles, & Wire ASTM B107 AZ31B 81 M11311 — Bar, Rods, Profiles, & Wire ASTM B107 AZ31B 81 M11311 — Bar, Rods, Profiles, & Wire ASTM B107 AZ31B 81 M11311 — Bar, Rods, Profiles, & Wire ASTM B107 AZ31B 81 M11311 — Hollow Profiles ASTM B107 AZ31B 81 M11311 — Tube ASTM B107 AZ31B 81 M11311 — Tube ASTM B107 AZ31C 81 M11312 — Tube ASTM B107 AZ31C 81 M11312 — Bar, Rods, Profiles, & Wire
(Continued)
55 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM B107 AZ31C 81 M11312 — Bar, Rods, Profiles, & Wire ASTM B107 AZ31C 81 M11312 — Bar, Rods, Profiles, & Wire ASTM B107 AZ31C 81 M11312 — Bar, Rods, Profiles, & Wire ASTM B107 AZ31C 81 M11312 — Tube ASTM B107 AZ31C 81 M11312 — Hollow Profiles ASTM B107 AZ61A 81 M11610 — Hollow Profiles ASTM B107 AZ61A 81 M11610 — Bar, Rods, Profiles, & Wire ASTM B107 AZ61A 81 M11610 — Bar, Rods, Profiles, & Wire ASTM B107 AZ61A 81 M11610 — Tube ASTM B107 AZ61A 81 M11610 — Bar, Rods, Profiles, & Wire ASTM B107 M1A 81 M15100 — Tube ASTM B107 M1A 81 M15100 — Bar, Rods, Profiles, & Wire ASTM B107 M1A 81 M15100 — Bar, Rods, Profiles, & Wire ASTM B107 M1A 81 M15100 — Bar, Rods, Profiles, & Wire ASTM B107 M1A 81 M15100 — Hollow Profiles ASTM/ASME B/SB-108 308.0 26 A03080 25 Castings ASTM/ASME B/SB-108 319.0 26 A03190 25 Castings ASTM/ASME B/SB-108 333.0, F 26 A03330 25 Castings ASTM/ASME B/SB-108 333.0, T5 26 A03330 25 Castings ASTM/ASME B/SB-108 333.0, T6 26 A03330 25 Castings ASTM/ASME B/SB-108 333.0, T7 26 A03330 25 Castings ASTM/ASME B/SB-108 356.0, F 26 A03560 24.2 Castings ASTM/ASME B/SB-108 356.0, T6 26 A03560 24.2 Castings ASTM/ASME B/SB-108 356.0, T71 26 A03560 24.2 Castings ASTM/ASME B/SB-108 443.0 26 A04430 24.1 Castings ASTM/ASME B/SB-108 513.0 26 A05130 23.2 Castings ASTM/ASME B/SB-108 535.0 26 A05350 — Castings ASTM/ASME B/SB-108 A356.0 26 A13560 24.2 Castings ASTM/ASME B/SB-108 A444.0 26 A14440 24.1 Castings ASTM/ASME B/SB-108 B443.0 26 A24430 24.1 Castings ASTM/ASME B/SB-111 — 31 C10100 31 Seamless Tube ASTM/ASME B/SB-111 — 31 C10200 31 Seamless Tube ASTM/ASME B/SB-111 — 31 C10300 31 Seamless Tube ASTM/ASME B/SB-111 — 31 C10800 31 Seamless Tube ASTM/ASME B/SB-111 — 31 C12000 31 Seamless Tube ASTM/ASME B/SB-111 — 31 C12200 31 Seamless Tube ASTM/ASME B/SB-111 — 31 C14200 31 Seamless Tube ASTM/ASME B/SB-111 — 31 C19200 31 Seamless Tube ASTM/ASME B/SB-111 — 32 C23000 32.1 Seamless Tube ASTM/ASME B/SB-111 — 32 C28000 32.1 Seamless Tube ASTM/ASME B/SB-111 — 32 C44300 32.2 Seamless Tube ASTM/ASME B/SB-111 — 32 C44400 32.2 Seamless Tube ASTM/ASME B/SB-111 — 32 C44500 32.2 Seamless Tube ASTM/ASME B/SB-111 — 35 C60800 35 Seamless Tube
(Continued)
56 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-111 — 35 C61300 35 Seamless Tube ASTM/ASME B/SB-111 — 35 C61400 35 Seamless Tube ASTM/ASME B/SB-111 — 32 C68700 32.2 Seamless Tube ASTM/ASME B/SB-111 — 34 C70400 34 Seamless Tube ASTM/ASME B/SB-111 — 34 C70600 34 Seamless Tube ASTM/ASME B/SB-111 — 34 C71000 34 Seamless Tube ASTM/ASME B/SB-111 — 34 C71500 34 Seamless Tube ASTM/ASME B/SB-111 — 34 C71640 34 Seamless Tube ASTM/ASME B/SB-111 — 34 C72200 34 Seamless Tube ASTM/ASME B/SB-127 — 42 N04400 42 Plate, Sheet, & Strip ASTM/ASME B/SB-135 — 32 C22000 32.1 Seamless Tube ASTM/ASME B/SB-135 — 32 C23000 32.1 Seamless Tube ASTM/ASME B/SB-148 — 35 C95200 35 Castings ASTM/ASME B/SB-148 — 35 C95300 35 Castings ASTM/ASME B/SB-148 — 35 C95400 35 Castings ASTM/ASME B/SB-148 — 35 C95410 35 Castings ASTM/ASME B/SB-148 — 35 C95500 35 Castings ASTM/ASME B/SB-148 — 35 C95600 35 Castings ASTM/ASME B/SB-148 — 35 C95700 35 Castings ASTM/ASME B/SB-148 — 35 C95800 35 Castings ASTM/ASME B/SB-150 — 35 C61300 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C61300 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C61300 35 Bar & Rod (Hex & Oct) ASTM/ASME B/SB-150 — 35 C61300 35 Bar & Rod (Hex & Oct) ASTM/ASME B/SB-150 — 35 C61300 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C61300 35 Bar & Rod (Hex & Oct) ASTM/ASME B/SB-150 — 35 C61300 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C61400 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C61400 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C61400 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C61400 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C61900 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C61900 35 Shapes ASTM/ASME B/SB-150 — 35 C61900 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C61900 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C61900 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C61900 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C62300 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C62300 35 Shapes ASTM/ASME B/SB-150 — 35 C62300 35 Bar & Rod (Hex & Oct) ASTM/ASME B/SB-150 — 35 C62300 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C62300 35 Bar & Rod (Hex & Oct) ASTM/ASME B/SB-150 — 35 C62300 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C62300 35 Rod (Round)
(Continued)
57 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-150 — 35 C62300 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C62300 35 Bar & Rod (Hex & Oct) ASTM/ASME B/SB-150 — 35 C62400 35 Shapes ASTM/ASME B/SB-150 — 35 C62400 35 Bar & Rod (Hex & Oct) ASTM/ASME B/SB-150 — 35 C62400 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C62400 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C62400 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C62400 35 Rod (Round) ASTM/ASME B/SB-150 — 35 C63000 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C63000 35 Shapes ASTM/ASME B/SB-150 — 35 C63000 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C63000 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C63000 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C63020 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C63020 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C63020 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C63200 35 Bar, Rod, & Shapes ASTM/ASME B/SB-150 — 35 C64200 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C64200 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C64200 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C64200 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C64200 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C64200 35 Bar & Rod ASTM/ASME B/SB-150 — 35 C64200 35 Shapes ASTM/ASME B/SB-151 — 34 C70600 34 Rod & Bar ASTM/ASME B/SB-151 — 34 C71500 34 Sq Bar & Rod (Rnd, Hex, Oct) ASTM/ASME B/SB-151 — 34 C71500 34 Sq Bar & Rod (Rnd, Hex, Oct) ASTM/ASME B/SB-151 — 34 C71500 34 Sq Bar & Rod (Rnd, Hex, Oct) ASTM/ASME B/SB-151 — 34 C71500 34 Bar (Rect.) & Shapes ASTM/ASME B/SB-152 — 31 C10100 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C10200 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C10300 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C10400 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C10500 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C10700 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C10800 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C11000 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C12000 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C12200 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C12300 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C14200 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-152 — 31 C14420 31 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-160 — 41 N02200 41 Rod & Bar ASTM/ASME B/SB-160 — 41 N02201 41 Rod & Bar
(Continued)
58 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-161 — 41 N02200 41 Seamless Pipe & Tube ASTM/ASME B/SB-161 — 41 N02201 41 Seamless Pipe & Tube ASTM/ASME B/SB-162 — 41 N02200 41 Plate, Sheet, & Strip ASTM/ASME B/SB-162 — 41 N02201 41 Plate, Sheet, & Strip ASTM/ASME B/SB-163 — 41 N02200 41 Seamless Tube ASTM/ASME B/SB-163 — 41 N02201 41 Seamless Tube ASTM/ASME B/SB-163 — 42 N04400 42 Seamless Tube ASTM/ASME B/SB-163 — 43 N06025 43 Seamless Tube ASTM/ASME B/SB-163 — 46 N06045 45 Seamless Tube ASTM/ASME B/SB-163 — 43 N06600 43 Seamless Tube ASTM/ASME B/SB-163 — 43 N06601 43 Seamless Tube ASTM/ASME B/SB-163 — 43 N06690 43 Seamless Tube ASTM/ASME B/SB-163 — 45 N08120 45 Seamless Tube ASTM/ASME B/SB-163 — 45 N08800 45 Seamless Tube ASTM/ASME B/SB-163 — 45 N08801 45 Seamless Tube ASTM/ASME B/SB-163 — 45 N08810 45 Seamless Tube ASTM/ASME B/SB-163 — 45 N08811 45 Seamless Tube ASTM/ASME B/SB-163 — 45 N08825 45 Seamless Tube ASTM/ASME B/SB-164 — 42 N04400 42 Rod, Bar, & Wire ASTM/ASME B/SB-164 — 42 N04405 42 Rod, Bar, & Wire ASTM/ASME B/SB-165 — 42 N04400 42 Seamless Pipe & Tube ASTM/ASME B/SB-166 — 43 N06025 43 Rod, Bar, & Wire ASTM/ASME B/SB-166 — 46 N06045 45 Rod, Bar, & Wire ASTM/ASME B/SB-166 — 43 N06600 43 Rod, Bar, & Wire ASTM/ASME B/SB-166 — 43 N06601 43 Rod, Bar, & Wire ASTM/ASME B/SB-166 — 43 N06617 46 Rod, Bar, & Wire ASTM/ASME B/SB-166 — 43 N06690 43 Rod, Bar, & Wire ASTM/ASME B/SB-167 — 43 N06025 43 Seamless Pipe & Tube ASTM/ASME B/SB-167 — 46 N06045 45 Seamless Pipe & Tube ASTM/ASME B/SB-167 — 43 N06600 43 Seamless Pipe & Tube ASTM/ASME B/SB-167 — 43 N06601 43 Seamless Pipe & Tube ASTM/ASME B/SB-167 — 43 N06617 46 Seamless Pipe & Tube ASTM/ASME B/SB-167 — 43 N06690 43 Seamless Pipe & Tube ASTM/ASME B/SB-168 — 43 N06025 43 Plate, Sheet, & Strip ASTM/ASME B/SB-168 — 46 N06045 45 Plate, Sheet, & Strip ASTM/ASME B/SB-168 — 43 N06600 43 Plate, Sheet, & Strip ASTM/ASME B/SB-168 — 43 N06601 43 Plate, Sheet, & Strip ASTM/ASME B/SB-168 — 43 N06617 46 Plate, Sheet, & Strip ASTM/ASME B/SB-168 — 43 N06690 43 Plate, Sheet, & Strip ASTM/ASME B/SB-169 — 35 C61300 35 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-169 — 35 C61300 35 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-169 — 35 C61300 35 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-169 — 35 C61400 35 Plate, Sheet, Strip, & Bar ASTM/ASME B/SB-169 — 35 C61400 35 Plate, Sheet, Strip, & Bar
(Continued)
59 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-169 — 35 C61400 35 Plate, Sheet, Strip, & Bar ASTM B170 1 31 C10100 31 Shapes ASTM B170 2 31 C10200 31 Shapes ASTM/ASME B/SB-171 — 32 C44300 32.2 Plate & Sheet ASTM/ASME B/SB-171 — 32 C44400 32.2 Plate & Sheet ASTM/ASME B/SB-171 — 32 C44500 32.2 Plate & Sheet ASTM/ASME B/SB-171 — 32 C46400 32.2 Plate & Sheet ASTM/ASME B/SB-171 — 32 C46500 32.2 Plate & Sheet ASTM/ASME B/SB-171 — 35 C61300 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C61300 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C61300 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C61400 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C61400 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C63000 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C63000 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C63000 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C63200 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C63200 35 Plate & Sheet ASTM/ASME B/SB-171 — 35 C63200 35 Plate & Sheet ASTM/ASME B/SB-171 — 34 C70600 34 Plate & Sheet ASTM/ASME B/SB-171 — 34 C71500 34 Plate & Sheet ASTM/ASME B/SB-171 — 34 C71500 34 Plate & Sheet ASTM/ASME B/SB-171 — 34 C72200 34 Plate & Sheet ASTM A182 F904L 45 N08904 8.2 Forgings ASTM/ASME B/SB-187 — 31 C10100 31 Rod & Bar ASTM/ASME B/SB-187 — 31 C10200 31 Rod & Bar ASTM/ASME B/SB-187 — 31 C10300 31 Rod & Bar ASTM/ASME B/SB-187 — 31 C10400 31 Rod & Bar ASTM/ASME B/SB-187 — 31 C10700 31 Rod & Bar ASTM/ASME B/SB-187 — 31 C10940 31 Rod & Bar ASTM/ASME B/SB-187 — 31 C11000 31 Rod & Bar ASTM/ASME B/SB-187 — 31 C14420 31 Rod & Bar ASTM B199 AM100A 83 M10100 — Castings ASTM B199 AZ91C, F 83 M11914 — Castings ASTM B199 AZ92A, F 83 M11920 — Castings ASTM/ASME B/SB-209 1060 21 A91060 21 Plate & Sheet ASTM/ASME B/SB-209 1100 21 A91100 21 Plate & Sheet ASTM/ASME B/SB-209 2014 24 A92014 26 Plate & Sheet ASTM/ASME B/SB-209 2219 24 A92219 26 Plate & Sheet ASTM/ASME B/SB-209 3003 21 A93003 22.1 Plate & Sheet ASTM/ASME B/SB-209 3004 22 A93004 22.2 Plate & Sheet ASTM/ASME B/SB-209 3005 22 A93005 22.2 Plate & Sheet ASTM/ASME B/SB-209 3105 22 A93105 22.2 Plate & Sheet ASTM/ASME B/SB-209 5005 22 A95005 22.2 Plate & Sheet
(Continued)
60 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-209 5010 22 A95010 22.2 Plate & Sheet ASTM/ASME B/SB-209 5050 21 A95050 22.2 Plate & Sheet ASTM/ASME B/SB-209 5052 22 A95052 22.3 Plate & Sheet ASTM/ASME B/SB-209 5083 25 A95083 22.4 Plate & Sheet ASTM/ASME B/SB-209 5083 25 A95083 22.4 Plate & Sheet ASTM/ASME B/SB-209 5083 25 A95083 22.4 Plate & Sheet ASTM/ASME B/SB-209 5083 25 A95083 22.4 Plate & Sheet ASTM/ASME B/SB-209 5083 25 A95083 22.4 Plate & Sheet ASTM/ASME B/SB-209 5086 25 A95086 22.4 Plate & Sheet ASTM/ASME B/SB-209 5154 22 A95154 22.4 Plate & Sheet ASTM/ASME B/SB-209 5252 22 A95252 22.3 Plate & Sheet ASTM/ASME B/SB-209 5254 22 A95254 22.4 Plate & Sheet ASTM/ASME B/SB-209 5454 22 A95454 22.3 Plate & Sheet ASTM/ASME B/SB-209 5456 25 A95456 22.4 Plate & Sheet ASTM/ASME B/SB-209 5456 25 A95456 22.4 Plate & Sheet ASTM/ASME B/SB-209 5456 25 A95456 22.4 Plate & Sheet ASTM/ASME B/SB-209 5456 25 A95456 22.4 Plate & Sheet ASTM/ASME B/SB-209 5456 25 A95456 22.4 Plate & Sheet ASTM/ASME B/SB-209 5457 22 A95457 22.2 Plate & Sheet ASTM/ASME B/SB-209 5652 22 A95652 22.3 Plate & Sheet ASTM/ASME B/SB-209 6061 23 A96061 23.1 Plate & Sheet ASTM/ASME B/SB-209 Alclad 2014 24 A82014 — Plate & Sheet ASTM/ASME B/SB-209 Alclad 2219 24 A82219 — Plate & Sheet ASTM/ASME B/SB-209 Alclad 3003 21 — — Plate & Sheet ASTM/ASME B/SB-209 Alclad 3003 21 — — Plate & Sheet ASTM/ASME B/SB-209 Alclad 3003 21 A83003 — Plate & Sheet ASTM/ASME B/SB-209 Alclad 3003 21 A83003 — Plate & Sheet ASTM/ASME B/SB-209 Alclad 3004 22 — — Plate & Sheet ASTM/ASME B/SB-209 Alclad 3004 22 — — Plate & Sheet ASTM/ASME B/SB-209 Alclad 3004 22 — — Plate & Sheet ASTM/ASME B/SB-209 Alclad 3004 22 — — Plate & Sheet ASTM/ASME B/SB-209 Alclad 6061 23 — — Plate & Sheet ASTM/ASME B/SB-209 Alclad 6061 23 A86061 — Plate & Sheet ASTM/ASME B/SB-209 Alclad 6061 23 A86061 — Plate & Sheet ASTM/ASME B/SB-210 1060 21 A91060 21 Seamless Tube ASTM B210 1100 21 A91100 21 Seamless Tube ASTM B210 2014 24 A92014 26 Seamless Tube ASTM/ASME B/SB-210 3003 21 A93003 22.1 Seamless Tube ASTM B210 3102 21 A93102 22.1 Seamless Tube ASTM B210 3303 21 A93303 — Seamless Tube ASTM B210 5005 22 A95005 22.2 Seamless Tube ASTM B210 5050 21 A95050 22.2 Seamless Tube ASTM/ASME B/SB-210 5052 22 A95052 22.3 Seamless Tube ASTM B210 5083 25 A95083 22.4 Seamless Tube
(Continued)
61 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM B210 5086 25 A95086 22.4 Seamless Tube ASTM/ASME B/SB-210 5154 22 A95154 22.4 Seamless Tube ASTM B210 5456 25 A95456 22.4 Seamless Tube ASTM/ASME B/SB-210 6061 23 A96061 23.1 Seamless Tube ASTM/ASME B/SB-210 6063 23 A96063 23.1 Seamless Tube ASTM/ASME B/SB-210 Alclad 3003 21 — — Seamless Tube ASTM B210 Alclad 3003 21 A83003 — Seamless Tube ASTM B210 Alclad 3102 21 — — Seamless Tube ASTM B210 Alclad 3303 21 — — Seamless Tube ASTM/ASME B/SB-211 1060 21 A91060 21 Bar, Rod, & Wire ASTM/ASME B/SB-211 1100 21 A91100 21 Bar, Rod, & Wire ASTM/ASME B/SB-211 2014 24 A92014 26 Bar, Rod, & Wire ASTM/ASME B/SB-211 2219 24 A92219 26 Bar, Rod, & Wire ASTM/ASME B/SB-211 3003 21 A93003 22.1 Bar, Rod, & Wire ASTM/ASME B/SB-211 5052 22 A95052 22.3 Bar, Rod, & Wire ASTM/ASME B/SB-211 5056 25 A95056 22.4 Bar, Rod, & Wire ASTM/ASME B/SB-211 5154 22 A95154 22.4 Bar, Rod, & Wire ASTM/ASME B/SB-211 6061 23 A96061 23.1 Bar, Rod, & Wire ASTM/ASME B/SB-211 Alclad 5056 25 — — Bar, Rod, & Wire ASTM/ASME B/SB-221 1060 21 A91060 21 Bar, Rod, & Shapes ASTM/ASME B/SB-221 1100 21 A91100 21 Bar, Rod, & Shapes ASTM/ASME B/SB-221 2014 24 A92014 26 Bar, Rod, & Shapes ASTM/ASME B/SB-221 2219 24 A92219 26 Bar, Rod, & Shapes ASTM/ASME B/SB-221 3003 21 A93003 22.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 3004 22 A93004 22.2 Bar, Rod, & Shapes ASTM/ASME B/SB-221 3102 21 A93102 22.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 5052 22 A95052 22.3 Bar, Rod, & Shapes ASTM/ASME B/SB-221 5083 25 A95083 22.4 Bar, Rod, & Shapes ASTM/ASME B/SB-221 5086 25 A95086 22.4 Bar, Rod, & Shapes ASTM/ASME B/SB-221 5154 22 A95154 22.4 Bar, Rod, & Shapes ASTM/ASME B/SB-221 5454 22 A95454 22.3 Bar, Rod, & Shapes ASTM/ASME B/SB-221 5456 25 A95456 22.4 Bar, Rod, & Shapes ASTM/ASME B/SB-221 6005 23 A96005 23.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 6005A 23 A96005 23.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 6061 23 A96061 23.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 6063 23 A96063 23.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 6105 23 A96105 23.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 6162 23 A96162 23.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 6351 23 A96351 23.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 6463 23 A96463 23.1 Bar, Rod, & Shapes ASTM/ASME B/SB-221 7005 27 A97005 23.2 Bar, Rod, & Shapes ASTM/ASME B/SB-221 Alclad 3003 21 A83003 — Bar, Rod, & Shapes ASTM B230 1350 21 A91350 21 Wire ASTM/ASME B/SB-234 1060 21 A91060 21 Seamless Tube
(Continued)
62 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-234 3003 21 A93003 22.1 Seamless Tube ASTM/ASME B/SB-234 5052 22 A95052 22.3 Seamless Tube ASTM/ASME B/SB-234 5454 22 A95454 22.3 Seamless Tube ASTM/ASME B/SB-234 6061 23 A96061 23.1 Seamless Tube ASTM/ASME B/SB-234 Alclad 3003 21 — — Seamless Tube ASTM/ASME B/SB-234 Alclad 3003 21 A83003 — Seamless Tube ASTM B236 1350 21 A91350 21 Bar ASTM A240 — 45 N08367 8.2 Sheet & Strip ASTM A240 — 45 N08367 8.2 Plate ASTM A240 904L 45 N08904 8.2 Plate, Sheet, & Strip ASTM/ASME B/SB-241 1060 21 A91060 21 Seamless Pipe & Tube ASTM/ASME B/SB-241 1100 21 A91100 21 Seamless Pipe & Tube ASTM/ASME B/SB-241 2014 24 A92014 26 Seamless Pipe & Tube ASTM/ASME B/SB-241 2219 24 A92219 26 Seamless Pipe & Tube ASTM/ASME B/SB-241 3003 21 A93003 22.1 Seamless Pipe & Tube ASTM/ASME B/SB-241 5052 22 A95052 22.3 Seamless Pipe & Tube ASTM/ASME B/SB-241 5083 25 A95083 22.4 Seamless Pipe & Tube ASTM/ASME B/SB-241 5086 25 A95086 22.4 Seamless Pipe & Tube ASTM/ASME B/SB-241 5454 22 A95454 22.3 Seamless Pipe & Tube ASTM/ASME B/SB-241 5456 25 A95456 22.4 Seamless Pipe & Tube ASTM/ASME B/SB-241 6061 23 A96061 23.1 Seamless Pipe & Tube ASTM/ASME B/SB-241 6063 23 A96063 23.1 Seamless Pipe & Tube ASTM/ASME B/SB-241 6162 23 A96162 23.1 Seamless Pipe & Tube ASTM/ASME B/SB-241 6351 23 A96351 23.1 Seamless Pipe & Tube ASTM/ASME B/SB-241 Alclad 3003 21 — — Seamless Pipe & Tube ASTM/ASME B/SB-241 Alclad 3003 21 A83003 — Seamless Pipe & Tube ASTM/ASME B/SB-247 1100 21 A91100 21 Forgings ASTM/ASME B/SB-247 2014 24 A92014 26 Forgings ASTM/ASME B/SB-247 2219 24 A92219 26 Forgings ASTM/ASME B/SB-247 3003 21 A93003 22.1 Forgings ASTM/ASME B/SB-247 5083 25 A95083 22.4 Forgings ASTM/ASME B/SB-247 6061 23 A96061 23.1 Forgings ASTM/ASME B/SB-247 6151 23 A96151 23.1 Forgings ASTM A249 — 45 N08367 8.2 Welded Tube ASTM A249 — 45 N08367 8.2 Welded Tube ASTM/ASME A/SA-249 — 45 N08904 8.2 Welded Tube ASTM/ASME B/SB-265 1 51 R50250 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 11 51 R52250 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 12 52 R53400 52 Plate, Sheet, & Strip ASTM/ASME B/SB-265 13 51 R53413 52 Plate, Sheet, & Strip ASTM/ASME B/SB-265 14 52 R53414 52 Plate, Sheet, & Strip ASTM/ASME B/SB-265 15 52 R53415 52 Plate, Sheet, & Strip ASTM/ASME B/SB-265 16 51 R52402 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 16H 51 R52402 51 Plate, Sheet, & Strip
(Continued)
63 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-265 17 51 R52252 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 18 53 R56322 53 Plate, Sheet, & Strip ASTM/ASME B/SB-265 19 53 R58640 54 Plate, Sheet, & Strip ASTM/ASME B/SB-265 2 51 R50400 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 20 53 R58645 54 Plate, Sheet, & Strip ASTM/ASME B/SB-265 21 53 R58210 54 Plate, Sheet, & Strip ASTM/ASME B/SB-265 24 54 R56405 53 Plate, Sheet, & Strip ASTM/ASME B/SB-265 25 54 R56403 53 Plate, Sheet, & Strip ASTM/ASME B/SB-265 26 51 R52404 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 26H 51 R52404 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 27 51 R52254 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 28 53 R56323 53 Plate, Sheet, & Strip ASTM/ASME B/SB-265 29 54 R56404 53 Plate, Sheet, & Strip ASTM/ASME B/SB-265 2H 51 R50400 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 3 52 R50550 52 Plate, Sheet, & Strip ASTM/ASME B/SB-265 30 51 R53530 52 Plate, Sheet, & Strip ASTM/ASME B/SB-265 31 52 R53532 52 Plate, Sheet, & Strip ASTM/ASME B/SB-265 32 53 R55111 52 Plate, Sheet, & Strip ASTM/ASME B/SB-265 33 51 R53442 54 Plate, Sheet, & Strip ASTM/ASME B/SB-265 34 52 R53445 54 Plate, Sheet, & Strip ASTM/ASME B/SB-265 35 54 R56340 53 Plate, Sheet, & Strip ASTM/ASME B/SB-265 4 53 R50700 51.4 Plate, Sheet, & Strip ASTM/ASME B/SB-265 5 54 R56400 53 Plate, Sheet, & Strip ASTM/ASME B/SB-265 6 54 R54520 52 Plate, Sheet, & Strip ASTM/ASME B/SB-265 7 51 R52400 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 7H 51 R52400 51 Plate, Sheet, & Strip ASTM/ASME B/SB-265 9 53 R56320 53 Plate, Sheet, & Strip ASTM/ASME B/SB-271 — 35 C95200 35 Castings ASTM/ASME B/SB-271 — 35 C95300 35 Castings ASTM/ASME B/SB-271 — 35 C95400 35 Castings ASTM/ASME B/SB-271 — 35 C95410 35 Castings ASTM/ASME B/SB-271 — 35 C95500 35 Castings ASTM B280 102 31 C10200 31 Seamless Tube ASTM B280 120 31 C12000 31 Seamless Tube ASTM B280 122 31 C12200 31 Seamless Tube ASTM/ASME B/SB-283 — 35 C64200 35 Forgings ASTM/ASME B/SB-283 — 35 C64200 35 Forgings ASTM/ASME B/SB-283 — 33 C65500 31 Forgings ASTM B302 — 31 C12000 31 Pipe ASTM B302 — 31 C12200 31 Pipe ASTM/ASME B/SB-308 6061 23 A96061 23.1 Shapes ASTM A312 — 45 N08904 8.2 Seamless & Welded Pipe ASTM A312 N08367 45 N08367 8.2 Seamless & Welded Pipe ASTM A312 N08367 45 N08367 8.2 Seamless & Welded Pipe
(Continued)
64 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM B313 1100 21 A91100 21 Welded Tube ASTM B313 3003 21 A93003 22.1 Welded Tube ASTM B313 3004 22 A93004 22.2 Welded Tube ASTM B313 3005 22 A93005 22.2 Welded Tube ASTM B313 5050 21 A95050 22.2 Welded Tube ASTM B313 5052 22 A95052 22.3 Welded Tube ASTM B313 5086 25 A95086 22.4 Welded Tube ASTM B313 5154 22 A95154 22.4 Welded Tube ASTM B313 6061 23 A96061 23.1 Welded Tube ASTM B313 Alclad 3004 22 — — Welded Tube ASTM/ASME B/SB-315 — 35 C61300 35 Seamless Pipe & Tube ASTM/ASME B/SB-315 — 35 C61400 35 Seamless Pipe & Tube ASTM/ASME B/SB-315 — 33 C65100 37 Seamless Pipe & Tube ASTM/ASME B/SB-315 — 33 C65500 33 Seamless Pipe & Tube ASTM B317 6101 23 A96101 23.1 Bar, Rod, Shapes, & Tube ASTM B324 1350 21 A91350 21 Wire ASTM/ASME B/SB-333 — 44 N10001 44 Plate, Sheet, & Strip ASTM/ASME B/SB-333 — 44 N10001 44 Plate, Sheet, & Strip ASTM/ASME B/SB-333 — 44 N10624 44 Plate, Sheet, & Strip ASTM/ASME B/SB-333 — 44 N10629 44 Plate, Sheet, & Strip ASTM/ASME B/SB-333 — 44 N10665 44 Plate, Sheet, & Strip ASTM/ASME B/SB-333 — 44 N10675 44 Plate, Sheet, & Strip ASTM/ASME B/SB-335 — 44 N10001 44 Rod ASTM/ASME B/SB-335 — 44 N10001 44 Rod ASTM/ASME B/SB-335 — 44 N10624 44 Rod ASTM/ASME B/SB-335 — 44 N10629 44 Rod ASTM/ASME B/SB-335 — 44 N10665 44 Rod ASTM/ASME B/SB-335 — 44 N10675 44 Rod ASTM B337 1 51 R50250 51 Seamless & Welded Pipe ASTM B337 11 51 R52250 51 Seamless & Welded Pipe ASTM B337 12 52 R53400 52 Seamless & Welded Pipe ASTM B337 2 51 R50400 51 Seamless & Welded Pipe ASTM B337 3 52 R50550 52 Seamless & Welded Pipe ASTM B337 7 51 R52400 51 Seamless & Welded Pipe ASTM B337 9 53 R56320 53 Seamless & Welded Pipe ASTM/ASME B/SB-338 1 51 R50250 51 Seamless & Welded Tube ASTM/ASME B/SB-338 11 51 R52250 51 Seamless & Welded Tube ASTM/ASME B/SB-338 12 52 R53400 52 Seamless & Welded Tube ASTM/ASME B/SB-338 13 51 R53413 52 Seamless & Welded Tube ASTM/ASME B/SB-338 14 52 R53414 52 Seamless & Welded Tube ASTM/ASME B/SB-338 15 52 R53415 52 Seamless & Welded Tube ASTM/ASME B/SB-338 16 51 R52402 51 Seamless & Welded Tube ASTM/ASME B/SB-338 16H 51 R52402 51 Seamless & Welded Tube ASTM/ASME B/SB-338 17 51 R52252 51 Seamless & Welded Tube
(Continued)
65 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-338 18 53 R56322 53 Seamless & Welded Tube ASTM/ASME B/SB-338 2 51 R50400 51 Seamless & Welded Tube ASTM/ASME B/SB-338 26 51 R52404 51 Seamless & Welded Tube ASTM/ASME B/SB-338 26H 51 R52404 51 Seamless & Welded Tube ASTM/ASME B/SB-338 27 51 R52254 51 Seamless & Welded Tube ASTM/ASME B/SB-338 28 53 R56323 53 Seamless & Welded Tube ASTM/ASME B/SB-338 2H 51 R50400 51 Seamless & Welded Tube ASTM/ASME B/SB-338 3 52 R50550 52 Seamless & Welded Tube ASTM/ASME B/SB-338 30 51 R53530 52 Seamless & Welded Tube ASTM/ASME B/SB-338 31 52 R53532 52 Seamless & Welded Tube ASTM/ASME B/SB-338 33 51 R53442 54 Seamless & Welded Tube ASTM/ASME B/SB-338 34 52 R53445 54 Seamless & Welded Tube ASTM/ASME B/SB-338 35 54 R56340 53 Seamless & Welded Tube ASTM/ASME B/SB-338 7 51 R52400 51 Seamless & Welded Tube ASTM/ASME B/SB-338 7H 51 R52400 51 Seamless & Welded Tube ASTM/ASME B/SB-338 9 53 R56320 53 Seamless & Welded Tube ASTM B345 1060 21 A91060 21 Seamless Pipe & Tube ASTM B345 3003 21 A93003 22.1 Seamless Pipe & Tube ASTM B345 5083 25 A95083 22.4 Seamless Pipe & Tube ASTM B345 5086 25 A95086 22.4 Seamless Pipe & Tube ASTM B345 6061 23 A96061 23.1 Seamless Pipe & Tube ASTM B345 6063 23 A96063 23.1 Seamless Pipe & Tube ASTM B345 6351 23 A96351 23.1 Seamless Pipe & Tube ASTM B345 Alclad 3003 21 A83003 — Seamless Pipe & Tube ASTM/ASME B/SB-348 1 51 R50250 51 Bars & Billets ASTM/ASME B/SB-348 11 51 R52250 51 Bars & Billets ASTM/ASME B/SB-348 12 52 R53400 52 Bars & Billets ASTM/ASME B/SB-348 13 51 R53413 52 Bars & Billets ASTM/ASME B/SB-348 14 52 R53414 52 Bars & Billets ASTM/ASME B/SB-348 15 52 R53415 52 Bars & Billets ASTM/ASME B/SB-348 16 51 R52402 51 Bars & Billets ASTM/ASME B/SB-348 16H 51 R52402 51 Bars & Billets ASTM/ASME B/SB-348 17 51 R52252 51 Bars & Billets ASTM/ASME B/SB-348 18 53 R56322 53 Bars & Billets ASTM/ASME B/SB-348 19 53 R58640 54 Bars & Billets ASTM/ASME B/SB-348 2 51 R50400 51 Bars & Billets ASTM/ASME B/SB-348 20 53 R58645 54 Bars & Billets ASTM/ASME B/SB-348 21 53 R58210 54 Bars & Billets ASTM/ASME B/SB-348 23 54 R56407 53 Bars & Billets ASTM/ASME B/SB-348 24 54 R56405 53 Bars & Billets ASTM/ASME B/SB-348 25 54 R56403 53 Bars & Billets ASTM/ASME B/SB-348 26 51 R52404 51 Bars & Billets ASTM/ASME B/SB-348 26H 51 R52404 51 Bars & Billets ASTM/ASME B/SB-348 28 53 R56323 53 Bars & Billets
(Continued)
66 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-348 2H 51 R50400 51 Bars & Billets ASTM/ASME B/SB-348 3 52 R50550 52 Bars & Billets ASTM/ASME B/SB-348 30 51 R53530 52 Bars & Billets ASTM/ASME B/SB-348 31 52 R53532 52 Bars & Billets ASTM/ASME B/SB-348 32 53 R55111 52 Bars & Billets ASTM/ASME B/SB-348 33 51 R53442 54 Bars & Billets ASTM/ASME B/SB-348 34 52 R53445 54 Bars & Billets ASTM/ASME B/SB-348 35 54 R56340 53 Bars & Billets ASTM/ASME B/SB-348 4 53 R50700 51.4 Bars & Billets ASTM/ASME B/SB-348 5 54 R56400 53 Bars & Billets ASTM/ASME B/SB-348 6 54 R54520 52 Bars & Billets ASTM/ASME B/SB-348 7 51 R52400 51 Bars & Billets ASTM/ASME B/SB-348 7H 51 R52400 51 Bars & Billets ASTM/ASME B/SB-348 9 53 R56320 53 Bars & Billets ASTM/ASME A/SA-351 CN7M 45 N08007 8.2 Castings ASTM/ASME A/SA-351 CT15C 45 N08151 45 Castings ASTM B351 R60001 61 R60001 61 Bar, Rod, & Wire ASTM B351 R60802 61 R60802 61 Bar, Rod, & Wire ASTM B351 R60804 61 R60804 61 Bar, Rod, & Wire ASTM B351 R60901 62 R60901 62 Bar, Rod, & Wire ASTM B353 R60001 61 R60001 61 Plate, Sheet, & Strip ASTM B352 R60802 61 R60802 61 Plate, Sheet, & Strip ASTM B352 R60804 61 R60804 61 Sheet & Strip ASTM B352 R60804 61 R60804 61 Plate ASTM B352 R60901 62 R60901 62 Plate, Sheet, & Strip ASTM B353 R60001 61 R60001 61 Seamless & Welded Tube ASTM B353 R60802 61 R60802 61 Seamless & Welded Tube ASTM B353 R60804 61 R60804 61 Seamless & Welded Tube ASTM B353 R60901 62 R60901 62 Seamless & Welded Tube ASTM B353 R60904 62 R60904 62 Seamless & Welded Tube ASTM A358 N08367 45 N08367 8.2 Fusion Welded Pipe ASTM A358 N08367 45 N08367 8.2 Fusion Welded Pipe ASTM B359 — 31 C10100 31 Seamless Tube ASTM B359 — 31 C10200 31 Seamless Tube ASTM B359 — 31 C10300 31 Seamless Tube ASTM B359 — 31 C10800 31 Seamless Tube ASTM B359 — 31 C12000 31 Seamless Tube ASTM/ASME B/SB-359 — 31 C12200 31 Seamless Tube ASTM B359 — 31 C14200 31 Seamless Tube ASTM B359 — 31 C19200 31 Seamless Tube ASTM B359 — 32 C23000 32.1 Seamless Tube ASTM/ASME B/SB-359 — 32 C44300 32.2 Seamless Tube ASTM/ASME B/SB-359 — 32 C44400 32.2 Seamless Tube ASTM/ASME B/SB-359 — 32 C44500 32.2 Seamless Tube
(Continued)
67 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM B359 — 35 C60800 35 Seamless Tube ASTM B359 — 32 C68700 32.2 Seamless Tube ASTM B359 — 34 C70400 34 Seamless Tube ASTM/ASME B/SB-359 — 34 C70600 34 Seamless Tube ASTM/ASME B/SB-359 — 34 C71000 34 Seamless Tube ASTM/ASME B/SB-359 — 34 C71500 34 Seamless Tube ASTM B359 — 34 C72200 34 Seamless Tube ASTM B361 5083 25 A95083 22.4 Fittings ASTM B361 5154 22 A95154 22.3 Fittings ASTM B361 WP Alclad 3003 21 A83003 — Fittings ASTM B361 WP1060 21 A91060 21 Fittings ASTM B361 WP1100 21 A91100 21 Fittings ASTM B361 WP3003 21 A93003 22.1 Fittings ASTM B361 WP6061 23 A96061 23.1 Fittings ASTM B361 WP6063 23 A96063 23.1 Fittings ASTM/ASME B/SB-363 WPT 1 51 R50250 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 11 51 R52250 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 12 52 R53400 52 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 13 51 R53413 52 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 14 52 R53414 52 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 15 52 R53415 52 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 16 51 R52402 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 16H 51 R52402 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 17 51 R52252 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 18 53 R56322 53 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 19 53 R58640 54 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 2 51 R50400 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 20 53 R58645 54 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 21 53 R58210 54 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 23 54 R56407 53 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 24 54 R56405 53 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 25 54 R56403 53 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 26 51 R52404 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 26H 51 R52404 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 28 53 R56323 53 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 3 52 R50550 52 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 30 51 R53530 52 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 7 51 R52400 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 7H 51 R52400 51 Seamless & Welded Fittings ASTM/ASME B/SB-363 WPT 9 53 R56320 53 Seamless & Welded Fittings ASTM/ASME B/SB-366 — 41 N02200 41 Fittings ASTM/ASME B/SB-366 — 41 N02201 41 Fittings ASTM/ASME B/SB-366 — 42 N04400 42 Fittings ASTM/ASME B/SB-366 — 43 N06002 43 Fittings
(Continued)
68 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-366 — 45 N06007 43 Fittings ASTM/ASME B/SB-366 — 43 N06022 44 Fittings ASTM/ASME B/SB-366 — 43 N06025 43 Fittings ASTM/ASME B/SB-366 — 45 N06030 45 Fittings ASTM/ASME B/SB-366 — 43 N06035 43 Fittings ASTM/ASME B/SB-366 — 46 N06045 45 Fittings ASTM/ASME B/SB-366 — 43 N06059 43 Fittings ASTM/ASME B/SB-366 — 43 N06200 43 Fittings ASTM/ASME B/SB-366 — 43 N06210 43 Fittings ASTM/ASME B/SB-366 — 43 N06230 43 Fittings ASTM/ASME B/SB-366 — 43 N06455 43 Fittings ASTM/ASME B/SB-366 — 43 N06600 43 Fittings ASTM/ASME B/SB-366 — 43 N06603 43 Fittings ASTM/ASME B/SB-366 — 43 N06625 43 Fittings ASTM/ASME B/SB-366 — 45 N06985 45 Fittings ASTM/ASME B/SB-366 — 45 N08020 45 Fittings ASTM/ASME B/SB-366 — 45 N08031 45 Fittings ASTM/ASME B/SB-366 — 45 N08120 45 Fittings ASTM/ASME B/SB-366 — 46 N08330 45 Fittings ASTM/ASME B/SB-366 — 45 N08367 8.2 Fittings ASTM/ASME B/SB-366 — 45 N08367 8.2 Fittings ASTM/ASME B/SB-366 — 45 N08800 45 Fittings ASTM/ASME B/SB-366 — 45 N08810 45 Fittings ASTM/ASME B/SB-366 — 45 N08811 45 Fittings ASTM/ASME B/SB-366 — 45 N08825 45 Fittings ASTM/ASME B/SB-366 — 45 N08904 8.2 Fittings ASTM/ASME B/SB-366 — 45 N08925 8.2 Fittings ASTM/ASME B/SB-366 — 45 N08926 8.2 Fittings ASTM/ASME B/SB-366 — 44 N10001 44 Fittings ASTM/ASME B/SB-366 — 44 N10003 44 Fittings ASTM/ASME B/SB-366 — 44 N10242 44 Fittings ASTM/ASME B/SB-366 — 43 N10276 43 Fittings ASTM/ASME B/SB-366 — 44 N10624 44 Fittings ASTM/ASME B/SB-366 — 44 N10629 44 Fittings ASTM/ASME B/SB-366 — 44 N10665 44 Fittings ASTM/ASME B/SB-366 — 44 N10675 44 Fittings ASTM/ASME B/SB-366 — 46 N12160 46 Fittings ASTM/ASME B/SB-366 — 45 R20033 45 Fittings ASTM/ASME B/SB-366 — 45 R30556 45 Fittings ASTM/ASME B/SB-367 C-16 51 R52402 51 Castings ASTM/ASME B/SB-367 C-17 51 R52252 51 Castings ASTM/ASME B/SB-367 C-2 51 R50400 51 Castings ASTM/ASME B/SB-367 C-3 52 R50550 52 Castings ASTM/ASME B/SB-367 C-5 54 R56400 53 Castings
(Continued)
69 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-367 C-6 54 R54520 52 Castings ASTM/ASME B/SB-367 C-7 51 — 51 Castings ASTM/ASME B/SB-367 C-8 52 — 52 Castings ASTM/ASME B/SB-369 — 34 C96200 34 Castings ASTM/ASME B/SB-381 F-1 51 R50250 51 Forgings ASTM/ASME B/SB-381 F-11 51 R52250 51 Forgings ASTM/ASME B/SB-381 F-12 52 R53400 52 Forgings ASTM/ASME B/SB-381 F-13 51 R53413 52 Forgings ASTM/ASME B/SB-381 F-14 52 R53414 52 Forgings ASTM/ASME B/SB-381 F-15 52 R53415 52 Forgings ASTM/ASME B/SB-381 F-16 51 R52402 51 Forgings ASTM/ASME B/SB-381 F-16H 51 R52402 51 Forgings ASTM/ASME B/SB-381 F-17 51 R52252 51 Forgings ASTM/ASME B/SB-381 F-18 53 R56322 53 Forgings ASTM/ASME B/SB-381 F-19 53 R58640 54 Forgings ASTM/ASME B/SB-381 F-2 51 R50400 51 Forgings ASTM/ASME B/SB-381 F-20 53 R58645 54 Forgings ASTM/ASME B/SB-381 F-21 53 R58210 54 Forgings ASTM/ASME B/SB-381 F-23 54 R56407 53 Forgings ASTM/ASME B/SB-381 F-24 54 R56405 53 Forgings ASTM/ASME B/SB-381 F-25 54 R56403 53 Forgings ASTM/ASME B/SB-381 F-26 51 R52404 51 Forgings ASTM/ASME B/SB-381 F-26H 51 R52404 51 Forgings ASTM/ASME B/SB-381 F-28 53 R56323 53 Forgings ASTM/ASME B/SB-381 F-2H 51 R50400 51 Forgings ASTM/ASME B/SB-381 F-3 52 R50550 52 Forgings ASTM/ASME B/SB-381 F-30 51 R53530 52 Forgings ASTM/ASME B/SB-381 F-31 52 R53532 52 Forgings ASTM/ASME B/SB-381 F-4 53 R50700 51.4 Forgings ASTM/ASME B/SB-381 F-5 54 R56400 53 Forgings ASTM/ASME B/SB-381 F-6 54 R54520 52 Forgings ASTM/ASME B/SB-381 F-7 51 R52400 51 Forgings ASTM/ASME B/SB-381 F-7H 51 R52400 51 Forgings ASTM/ASME B/SB-381 F-9 53 R56320 53 Forgings ASTM/ASME B/SB-395 — 31 C10200 31 Seamless Tube ASTM/ASME B/SB-395 — 31 C10300 31 Seamless Tube ASTM/ASME B/SB-395 — 31 C10800 31 Seamless Tube ASTM/ASME B/SB-395 — 31 C12000 31 Seamless Tube ASTM/ASME B/SB-395 — 31 C12200 31 Seamless Tube ASTM/ASME B/SB-395 — 31 C14200 31 Seamless Tube ASTM/ASME B/SB-395 — 31 C19200 31 Seamless Tube ASTM/ASME B/SB-395 — 32 C23000 32.1 Seamless Tube ASTM/ASME B/SB-395 — 32 C44300 32.2 Seamless Tube ASTM/ASME B/SB-395 — 32 C44400 32.2 Seamless Tube
(Continued)
70 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-395 — 32 C44500 32.2 Seamless Tube ASTM/ASME B/SB-395 — 35 C60800 35 Seamless Tube ASTM/ASME B/SB-395 — 32 C68700 32.2 Seamless Tube ASTM/ASME B/SB-395 — 34 C70400 34 Seamless Tube ASTM/ASME B/SB-395 — 34 C70600 34 Seamless Tube ASTM/ASME B/SB-395 — 34 C71000 34 Seamless Tube ASTM/ASME B/SB-395 — 34 C71500 34 Seamless Tube ASTM/ASME B/SB-395 — 34 C72200 34 Seamless Tube ASTM B396 5005 22 A95005 22.2 Wire ASTM B403 AM100A, F 83 M10100 — Castings ASTM B403 AZ91C, F 83 M11914 — Castings ASTM B403 AZ92A, F 83 M11920 — Castings ASTM B403 K1A 83 M18010 — Castings ASTM/ASME B/SB-407 — 45 N08120 45 Seamless Pipe & Tube ASTM/ASME B/SB-407 — 45 N08800 45 Seamless Pipe & Tube ASTM/ASME B/SB-407 — 45 N08801 45 Seamless Pipe & Tube ASTM/ASME B/SB-407 — 45 N08810 45 Seamless Pipe & Tube ASTM/ASME B/SB-407 — 45 N08811 45 Seamless Pipe & Tube ASTM/ASME B/SB-408 — 45 N08120 45 Rod & Bar ASTM/ASME B/SB-408 — 45 N08800 45 Rod & Bar ASTM/ASME B/SB-408 — 45 N08810 45 Rod & Bar ASTM/ASME B/SB-408 — 45 N08811 45 Rod & Bar ASTM/ASME B/SB-409 — 45 N08120 45 Plate, Sheet, & Strip ASTM/ASME B/SB-409 — 45 N08800 45 Plate, Sheet, & Strip ASTM/ASME B/SB-409 — 45 N08810 45 Plate, Sheet, & Strip ASTM/ASME B/SB-409 — 45 N08811 45 Plate, Sheet, & Strip ASTM/ASME B/SB-423 — 45 N08221 45 Seamless Pipe & Tube ASTM/ASME B/SB-423 — 45 N08825 45 Seamless Pipe & Tube ASTM/ASME B/SB-424 — 45 N08221 45 Plate, Sheet, & Strip ASTM/ASME B/SB-424 — 45 N08825 45 Plate, Sheet, & Strip ASTM/ASME B/SB-425 — 45 N08221 45 Rod & Bar ASTM/ASME B/SB-425 — 45 N08825 45 Rod & Bar ASTM B429 6061 23 A96061 23.1 Pipe & Tube ASTM B429 6063 23 A96063 23.1 Pipe & Tube ASTM/ASME B/SB-434 — 44 N10003 44 Plate, Sheet, & Strip ASTM/ASME B/SB-434 — 44 N10242 44 Plate, Sheet, & Strip ASTM/ASME B/SB-435 — 43 N06002 43 Plate, Sheet, & Strip ASTM/ASME B/SB-435 — 43 N06230 43 Plate, Sheet, & Strip ASTM/ASME B/SB-435 — 46 N12160 46 Plate, Sheet, & Strip ASTM/ASME B/SB-435 — 45 R30556 45 Plate, Sheet, & Strip ASTM/ASME B/SB-443 1 43 N06625 43 Plate, Sheet, & Strip ASTM/ASME B/SB-443 2 43 N06625 43 Plate, Sheet, & Strip ASTM/ASME B/SB-444 1 43 N06625 43 Seamless Pipe & Tube ASTM/ASME B/SB-444 2 43 N06625 43 Seamless Pipe & Tube
(Continued)
71 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-446 1 43 N06625 43 Rod & Bar ASTM/ASME B/SB-446 2 43 N06625 43 Rod & Bar ASTM/ASME B/SB-462 — 43 N06022 44 Forgings ASTM/ASME B/SB-462 — 45 N06030 45 Forgings ASTM/ASME B/SB-462 — 43 N06035 43 Forgings ASTM/ASME B/SB-462 — 46 N06045 45 Forgings ASTM/ASME B/SB-462 — 43 N06059 43 Forgings ASTM/ASME B/SB-462 — 43 N06200 43 Forgings ASTM/ASME B/SB-462 — 43 N06686 43 Forgings ASTM/ASME B/SB-462 — 45 N08020 45 Forgings ASTM/ASME B/SB-462 — 45 N08024 45 Forgings ASTM/ASME B/SB-462 — 45 N08026 45 Forgings ASTM/ASME B/SB-462 — 45 N08031 45 Forgings ASTM/ASME B/SB-462 — 45 N08367 8.2 Forgings ASTM/ASME B/SB-462 — 43 N10276 43 Forgings ASTM/ASME B/SB-462 — 44 N10629 44 Forgings ASTM/ASME B/SB-462 — 44 N10665 44 Forgings ASTM/ASME B/SB-462 — 44 N10675 44 Forgings ASTM/ASME B/SB-462 — 45 R20033 45 Forgings ASTM/ASME B/SB-463 — 45 N08020 45 Plate, Sheet, & Strip ASTM/ASME B/SB-463 — 45 N08024 45 Plate, Sheet, & Strip ASTM/ASME B/SB-463 — 45 N08026 45 Plate, Sheet, & Strip ASTM/ASME B/SB-464 — 45 N08020 45 Welded Pipe ASTM/ASME B/SB-464 — 45 N08024 45 Welded Pipe ASTM/ASME B/SB-464 — 45 N08026 45 Welded Pipe ASTM/ASME B/SB-466 — 34 C70400 34 Seamless Pipe & Tube ASTM/ASME B/SB-466 — 34 C70600 34 Seamless Pipe & Tube ASTM/ASME B/SB-466 — 34 C71000 34 Seamless Pipe & Tube ASTM/ASME B/SB-466 — 34 C71500 34 Seamless Pipe & Tube ASTM/ASME B/SB-466 — 34 C72200 34 Seamless Pipe & Tube ASTM/ASME B/SB-467 — 34 C70600 34 Welded Pipe ASTM/ASME B/SB-467 — 34 C70600 34 Welded Pipe ASTM/ASME B/SB-467 — 34 C71500 34 Welded Pipe ASTM/ASME B/SB-467 — 34 C71500 34 Welded Pipe ASTM/ASME B/SB-468 — 45 N08020 45 Welded Tube ASTM/ASME B/SB-468 — 45 N08024 45 Welded Tube ASTM/ASME B/SB-468 — 45 N08026 45 Welded Tube ASTM/ASME B/SB-473 — 45 N08020 45 Bar ASTM/ASME B/SB-473 — 45 N08024 45 Bar ASTM/ASME B/SB-473 — 45 N08026 45 Bar ASTM A479 904L 45 N08904 8.2 Bars & Shapes ASTM B483 1060 21 A91060 21 Tube ASTM B483 1100 21 A91100 21 Tube ASTM B483 1435 21 A91435 21 Tube
(Continued)
72 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM B483 3003 21 A93003 22.1 Tube ASTM B483 3102 21 A93102 22.1 Tube ASTM B483 5005 22 A95005 22.2 Tube ASTM B483 5050 21 A95050 22.2 Tube ASTM B483 5052 22 A95052 22.3 Tube ASTM B483 6061 23 A96061 23.1 Tube ASTM B483 6063 23 A96063 23.1 Tube ASTM B491 1050 21 A91050 21 Extruded Tube ASTM B491 1100 21 A91100 21 Extruded Tube ASTM B491 1200 21 A91200 21 Extruded Tube ASTM B491 1235 21 A91235 21 Extruded Tube ASTM B491 3003 21 A93003 22.1 Extruded Tube ASTM B491 3102 21 A93102 22.1 Extruded Tube ASTM B491 6063 23 A96063 23.1 Extruded Tube ASTM/ASME B/SB-493 R60702 61 R60702 61 Forgings ASTM/ASME B/SB-493 R60704 62 R60704 62 Forgings ASTM/ASME B/SB-493 R60705 62 R60705 62 Forgings ASTM/ASME A/SA-494 CU5MCuC 45 N08826 45 Castings ASTM/ASME A/SA-494 CW2M 43 N26455 43 Castings ASTM/ASME A/SA-494 CW6M 44 N30107 44 Castings ASTM/ASME A/SA-494 CW6MC 43 N26625 43 Castings ASTM/ASME A/SA-494 CX2MW 43 N26022 44 Castings ASTM/ASME A/SA-494 CY40 43 N06040 43 Castings ASTM/ASME A/SA-494 M30C 42 N24130 42 Castings ASTM/ASME A/SA-494 M35-1 42 N24135 42 Castings ASTM/ASME A/SA-494 M35-2 42 N04020 42 Castings ASTM/ASME A/SA-494 N7M 44 N30007 44 Castings ASTM/ASME B/SB-505 — 35 C95200 35 Castings ASTM/ASME B/SB-511 — 46 N08330 45 Bars & Shapes ASTM/ASME B/SB-511 — 46 N08332 45 Bars & Shapes ASTM B512 — 46 N08330 45 Bars & Billets ASTM/ASME B/SB-514 — 45 N08120 45 Welded Pipe ASTM/ASME B/SB-514 — 45 N08800 45 Welded Pipe ASTM/ASME B/SB-514 — 45 N08810 45 Welded Pipe ASTM/ASME B/SB-515 — 45 N08120 45 Welded Tube ASTM/ASME B/SB-515 — 45 N08800 45 Welded Tube ASTM/ASME B/SB-515 — 45 N08810 45 Welded Tube ASTM/ASME B/SB-515 — 45 N08811 45 Welded Tube ASTM/ASME B/SB-516 — 43 N06025 43 Welded Tube ASTM/ASME B/SB-516 — 46 N06045 45 Welded Tube ASTM/ASME B/SB-516 — 43 N06600 43 Welded Tube ASTM/ASME B/SB-516 — 43 N06603 43 Welded Tube ASTM/ASME B/SB-517 — 43 N06025 43 Welded Pipe ASTM/ASME B/SB-517 — 46 N06045 45 Welded Pipe
(Continued)
73 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-517 — 43 N06600 43 Welded Pipe ASTM/ASME B/SB-517 — 43 N06603 43 Welded Pipe ASTM/ASME B/SB-523 R60702 61 R60702 61 Seamless & Welded Tube ASTM/ASME B/SB-523 R60704 62 R60704 62 Seamless & Welded Tube ASTM/ASME B/SB-523 R60705 62 R60705 62 Seamless & Welded Tube ASTM/ASME B/SB-535 — 46 N08330 45 Seamless Pipe & Tube ASTM/ASME B/SB-535 — 46 N08332 45 Seamless Pipe & Tube ASTM/ASME B/SB-536 — 46 N08330 45 Plate, Sheet, & Strip ASTM/ASME B/SB-536 — 46 N08332 45 Plate, Sheet, & Strip ASTM/ASME B/SB-543 — 31 C10800 31 Welded Tube ASTM/ASME B/SB-543 — 31 C12200 31 Welded Tube ASTM/ASME B/SB-543 — 31 C19400 31 Welded Tube ASTM/ASME B/SB-543 — 32 C23000 32.1 Welded Tube ASTM/ASME B/SB-543 — 32 C44300 32.2 Welded Tube ASTM/ASME B/SB-543 — 32 C44400 32.2 Welded Tube ASTM/ASME B/SB-543 — 32 C44500 32.2 Welded Tube ASTM/ASME B/SB-543 — 32 C68700 32.2 Welded Tube ASTM/ASME B/SB-543 — 34 C70400 34 Welded Tube ASTM/ASME B/SB-543 — 34 C70600 34 Welded Tube ASTM B543 — 34 C71000 34 Welded Tube ASTM/ASME B/SB-543 — 34 C71500 34 Welded Tube ASTM/ASME B/SB-543 — 34 C71640 34 Welded Tube ASTM B543 — 34 C72200 34 Welded Tube ASTM B547 1100 21 A91100 21 Welded Tube ASTM B547 3003 21 A93003 22.1 Welded Tube ASTM B547 3004 22 A93004 22.2 Welded Tube ASTM B547 5050 21 A95050 22.2 Welded Tube ASTM B547 5052 22 A95052 22.3 Welded Tube ASTM B547 5083 25 A95083 22.4 Welded Tube ASTM B547 5086 25 A95086 22.4 Welded Tube ASTM B547 5154 22 A95154 22.4 Welded Tube ASTM B547 5454 22 A95454 22.3 Welded Tube ASTM B547 6061 23 A96061 23.1 Welded Tube ASTM B547 Alclad 3003 21 A83003 — Welded Tube ASTM B547 Alclad 3004 22 — — Welded Tube ASTM/ASME B/SB-550 R60702 61 R60702 61 Bar & Wire ASTM/ASME B/SB-550 R60704 62 R60704 62 Bar & Wire ASTM/ASME B/SB-550 R60705 62 R60705 62 Bar & Wire ASTM/ASME B/SB-551 R60702 61 R60702 61 Plate, Sheet, & Strip ASTM/ASME B/SB-551 R60704 62 R60704 62 Plate, Sheet, & Strip ASTM/ASME B/SB-551 R60705 62 R60705 62 Plate, Sheet, & Strip ASTM/ASME B/SB-551 R60706 62 R60706 62 Plate, Sheet, & Strip ASTM/ASME B/SB-564 — 41 N02200 41 Forgings ASTM/ASME B/SB-564 — 42 N04400 42 Forgings
(Continued)
74 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-564 — 43 N06022 44 Forgings ASTM/ASME B/SB-564 — 43 N06025 43 Forgings ASTM/ASME B/SB-564 — 43 N06025 43 Forgings ASTM/ASME B/SB-564 — 43 N06035 43 Forgings ASTM/ASME B/SB-564 — 46 N06045 45 Forgings ASTM/ASME B/SB-564 — 43 N06059 43 Forgings ASTM/ASME B/SB-564 — 43 N06110 43 Forgings ASTM/ASME B/SB-564 — 43 N06110 43 Forgings ASTM/ASME B/SB-564 — 43 N06200 43 Forgings ASTM/ASME B/SB-564 — 43 N06210 43 Forgings ASTM/ASME B/SB-564 — 43 N06230 43 Forgings ASTM/ASME B/SB-564 — 43 N06600 43 Forgings ASTM/ASME B/SB-564 — 43 N06603 43 Forgings ASTM/ASME B/SB-564 — 43 N06617 46 Forgings ASTM/ASME B/SB-564 — 43 N06625 43 Forgings ASTM/ASME B/SB-564 — 43 N06625 43 Forgings ASTM/ASME B/SB-564 — 43 N06686 43 Forgings ASTM/ASME B/SB-564 — 43 N06690 43 Forgings ASTM/ASME B/SB-564 — 45 N08031 45 Forgings ASTM/ASME B/SB-564 — 45 N08120 45 Forgings ASTM/ASME B/SB-564 — 45 N08367 8.2 Forgings ASTM/ASME B/SB-564 — 45 N08800 45 Forgings ASTM/ASME B/SB-564 — 45 N08810 45 Forgings ASTM/ASME B/SB-564 — 45 N08811 44 Forgings ASTM/ASME B/SB-564 — 45 N08825 45 Forgings ASTM/ASME B/SB-564 — 44 N10242 44 Forgings ASTM/ASME B/SB-564 — 43 N10276 43 Forgings ASTM/ASME B/SB-564 — 44 N10624 44 Forgings ASTM/ASME B/SB-564 — 44 N10629 44 Forgings ASTM/ASME B/SB-564 — 44 N10665 44 Forgings ASTM/ASME B/SB-564 — 44 N10675 44 Forgings ASTM/ASME B/SB-564 — 46 N12160 46 Forgings ASTM/ASME B/SB-564 — 45 R20033 45 Forgings ASTM/ASME B/SB-572 — 43 N06002 43 Rod ASTM/ASME B/SB-572 — 43 N06230 43 Rod ASTM/ASME B/SB-572 — 46 N12160 46 Rod ASTM/ASME B/SB-572 — 45 R30556 45 Rod ASTM/ASME B/SB-573 — 44 N10003 44 Rod ASTM/ASME B/SB-573 — 44 N10242 44 Rod ASTM/ASME B/SB-574 — 43 N06022 44 Rod ASTM/ASME B/SB-574 — 43 N06035 43 Rod ASTM/ASME B/SB-574 — 43 N06059 43 Rod ASTM/ASME B/SB-574 — 43 N06200 43 Rod ASTM/ASME B/SB-574 — 43 N06210 43 Rod
(Continued)
75 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-574 — 43 N06455 43 Rod ASTM/ASME B/SB-574 — 43 N06686 43 Rod ASTM/ASME B/SB-574 — 43 N10276 43 Rod ASTM/ASME B/SB-575 — 43 N06022 44 Plate, Sheet, & Strip ASTM/ASME B/SB-575 — 43 N06035 43 Plate, Sheet, & Strip ASTM/ASME B/SB-575 — 43 N06059 43 Plate, Sheet, & Strip ASTM/ASME B/SB-575 — 43 N06200 43 Plate, Sheet, & Strip ASTM/ASME B/SB-575 — 43 N06210 43 Plate, Sheet, & Strip ASTM/ASME B/SB-575 — 43 N06455 43 Plate, Sheet, & Strip ASTM/ASME B/SB-575 — 43 N06686 43 Plate, Sheet, & Strip ASTM/ASME B/SB-575 — 43 N10276 43 Plate, Sheet, & Strip ASTM/ASME B/SB-581 — 45 N06007 43 Rod ASTM/ASME B/SB-581 — 45 N06007 43 Rod ASTM/ASME B/SB-581 — 45 N06030 45 Rod ASTM/ASME B/SB-581 — 45 N06975 45 Rod ASTM/ASME B/SB-581 — 45 N06985 45 Rod ASTM/ASME B/SB-581 — 45 N06985 45 Rod ASTM/ASME B/SB-581 — 45 N08031 45 Rod ASTM/ASME B/SB-582 — 45 N06007 43 Plate, Sheet, & Strip ASTM/ASME B/SB-582 — 45 N06007 43 Plate, Sheet, & Strip ASTM/ASME B/SB-582 — 45 N06030 45 Plate, Sheet, & Strip ASTM/ASME B/SB-582 — 45 N06975 45 Plate, Sheet, & Strip ASTM/ASME B/SB-582 — 45 N06985 45 Plate, Sheet, & Strip ASTM/ASME B/SB-582 — 45 N06985 45 Plate, Sheet, & Strip ASTM/ASME B/SB-599 — 45 N08700 8.2 Plate, Sheet, & Strip ASTM B608 — 35 C61300 35 Welded Pipe ASTM B608 — 35 C61400 35 Welded Pipe ASTM B608 — 34 C70620 34 Welded Pipe ASTM B608 — 34 C71520 34 Welded Pipe ASTM B609 1350 21 A91350 21 Wire ASTM B618 208.0 26 A02080 25 Castings ASTM B618 319.0 26 A03190 25 Castings ASTM B618 328.0 26 A03280 25 Castings ASTM B618 356.0 26 A03560 24.2 Castings ASTM B618 443.0 26 A04430 24.1 Castings ASTM B618 514.0 26 A05140 23.1 Castings ASTM B618 535.0 26 A05350 — Castings ASTM B618 A356.0 26 A13560 24.2 Castings ASTM B618 B443.0 26 A24430 24.1 Castings ASTM/ASME B/SB-619 — 43 N06002 43 Welded Pipe ASTM/ASME B/SB-619 — 45 N06007 43 Welded Pipe ASTM/ASME B/SB-619 — 43 N06022 44 Welded Pipe ASTM/ASME B/SB-619 — 45 N06030 45 Welded Pipe ASTM/ASME B/SB-619 — 43 N06035 43 Welded Pipe
(Continued)
76 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-619 — 43 N06059 43 Welded Pipe ASTM/ASME B/SB-619 — 43 N06200 43 Welded Pipe ASTM/ASME B/SB-619 — 43 N06210 43 Welded Pipe ASTM/ASME B/SB-619 — 43 N06230 43 Welded Pipe ASTM/ASME B/SB-619 — 43 N06455 43 Welded Pipe ASTM/ASME B/SB-619 — 43 N06686 43 Welded Pipe ASTM/ASME B/SB-619 — 45 N06975 45 Welded Pipe ASTM/ASME B/SB-619 — 45 N06985 45 Welded Pipe ASTM/ASME B/SB-619 — 45 N08031 45 Welded Pipe ASTM/ASME B/SB-619 — 45 N08320 8.2 Welded Pipe ASTM/ASME B/SB-619 — 44 N10001 44 Welded Pipe ASTM/ASME B/SB-619 — 44 N10242 44 Welded Pipe ASTM/ASME B/SB-619 — 43 N10276 43 Welded Pipe ASTM/ASME B/SB-619 — 44 N10624 44 Welded Pipe ASTM/ASME B/SB-619 — 44 N10629 44 Welded Pipe ASTM/ASME B/SB-619 — 44 N10665 44 Welded Pipe ASTM/ASME B/SB-619 — 44 N10675 44 Welded Pipe ASTM/ASME B/SB-619 — 46 N12160 46 Welded Pipe ASTM/ASME B/SB-619 — 45 R20033 45 Welded Pipe ASTM/ASME B/SB-619 — 45 R30556 45 Welded Pipe ASTM/ASME B/SB-620 — 45 N08320 8.2 Plate, Sheet, & Strip ASTM/ASME B/SB-621 — 45 N08320 8.2 Rod ASTM/ASME B/SB-622 — 43 N06002 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 N06007 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06022 44 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 N06030 45 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06035 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06059 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06060 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06200 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06210 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06230 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06250 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06255 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06455 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 43 N06686 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 N06975 45 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 N06985 45 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 N08031 45 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 N08135 45 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 N08320 8.2 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 N08535 45 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 44 N10001 44 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 44 N10242 44 Seamless Pipe & Tube
(Continued)
77 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-622 — 43 N10276 43 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 44 N10624 44 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 44 N10629 44 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 44 N10665 44 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 44 N10675 44 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 46 N12160 46 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 R20033 45 Seamless Pipe & Tube ASTM/ASME B/SB-622 — 45 R30556 45 Seamless Pipe & Tube ASTM/ASME B/SB-625 — 45 N08031 45 Plate, Sheet, & Strip ASTM/ASME B/SB-625 — 45 N08904 8.2 Plate, Sheet, & Strip ASTM/ASME B/SB-625 — 45 N08925 8.2 Plate, Sheet, & Strip ASTM/ASME B/SB-625 — 45 N08926 8.2 Plate, Sheet, & Strip ASTM/ASME B/SB-625 — 45 N08932 8.2 Plate, Sheet, & Strip ASTM/ASME B/SB-625 — 45 R20033 45 Plate, Sheet, & Strip ASTM/ASME B/SB-626 — 43 N06002 43 Welded Tube ASTM/ASME B/SB-626 — 45 N06007 43 Welded Tube ASTM/ASME B/SB-626 — 43 N06022 44 Welded Tube ASTM/ASME B/SB-626 — 45 N06030 45 Welded Tube ASTM/ASME B/SB-626 — 43 N06035 43 Welded Tube ASTM/ASME B/SB-626 — 43 N06059 43 Welded Tube ASTM/ASME B/SB-626 — 43 N06200 43 Welded Tube ASTM/ASME B/SB-626 — 43 N06210 43 Welded Tube ASTM/ASME B/SB-626 — 43 N06230 43 Welded Tube ASTM/ASME B/SB-626 — 43 N06455 43 Welded Tube ASTM/ASME B/SB-626 — 43 N06686 43 Welded Tube ASTM/ASME B/SB-626 — 45 N06975 45 Welded Tube ASTM/ASME B/SB-626 — 45 N06985 45 Welded Tube ASTM/ASME B/SB-626 — 45 N08031 45 Welded Tube ASTM/ASME B/SB-626 — 45 N08320 8.2 Welded Tube ASTM/ASME B/SB-626 — 44 N10001 44 Welded Tube ASTM/ASME B/SB-626 — 44 N10242 44 Welded Tube ASTM/ASME B/SB-626 — 43 N10276 43 Welded Tube ASTM/ASME B/SB-626 — 44 N10624 44 Welded Tube ASTM/ASME B/SB-626 — 44 N10629 44 Welded Tube ASTM/ASME B/SB-626 — 44 N10665 44 Welded Tube ASTM/ASME B/SB-626 — 44 N10675 44 Welded Tube ASTM/ASME B/SB-626 — 46 N12160 46 Welded Tube ASTM/ASME B/SB-626 — 45 R20033 45 Welded Tube ASTM/ASME B/SB-626 — 45 R30556 45 Welded Tube ASTM/ASME B/SB-649 — 45 N08031 45 Bar & Wire ASTM/ASME B/SB-649 — 45 N08904 8.2 Bar & Wire ASTM/ASME B/SB-649 — 45 N08925 8.2 Bar & Wire ASTM/ASME B/SB-649 — 45 N08926 8.2 Bar & Wire ASTM/ASME B/SB-649 — 45 R20033 45 Bar & Wire
(Continued)
78 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-653 R60702 61 R60702 61 Seamless & Welded Fittings ASTM/ASME B/SB-658 R60702 61 R60702 61 Seamless & Welded Pipe ASTM/ASME B/SB-658 R60704 62 R60704 62 Seamless & Welded Pipe ASTM/ASME B/SB-658 R60705 62 R60705 62 Seamless & Welded Pipe ASTM/ASME B/SB-668 — 45 N08028 45 Seamless Tube ASTM/ASME B/SB-672 — 45 N08700 8.2 Bar & Wire ASTM/ASME B/SB-673 — 45 N08904 8.2 Welded Pipe ASTM/ASME B/SB-673 — 45 N08925 8.2 Welded Pipe ASTM/ASME B/SB-673 — 45 N08926 8.2 Welded Pipe ASTM/ASME B/SB-674 — 45 N08904 8.2 Welded Tube ASTM/ASME B/SB-674 — 45 N08925 8.2 Welded Tube ASTM/ASME B/SB-674 — 45 N08926 8.2 Welded Tube ASTM/ASME B/SB-675 — 45 N08367 8.2 Welded Pipe ASTM/ASME B/SB-675 — 45 N08367 8.2 Welded Pipe ASTM/ASME B/SB-676 — 45 N08367 8.2 Welded Tube ASTM/ASME B/SB-676 — 45 N08367 8.2 Welded Tube ASTM/ASME B/SB-677 — 45 N08904 8.2 Seamless Pipe & Tube ASTM/ASME B/SB-677 — 45 N08925 8.2 Seamless Pipe & Tube ASTM/ASME B/SB-677 — 45 N08926 8.2 Seamless Pipe & Tube ASTM B686 A356.0 26 A13560 24.2 Castings ASTM/ASME B/SB-688 — 45 N08366 8.2 Plate, Sheet, & Strip ASTM/ASME B/SB-688 — 45 N08367 8.2 Plate, Sheet, & Strip ASTM/ASME B/SB-688 — 45 N08367 8.2 Plate, Sheet, & Strip ASTM/ASME B/SB-690 — 45 N08366 8.2 Seamless Pipe & Tube ASTM/ASME B/SB-690 — 45 N08367 8.2 Seamless Pipe & Tube ASTM/ASME B/SB-690 — 45 N08367 8.2 Seamless Pipe & Tube ASTM/ASME B/SB-691 — 45 N08366 8.2 Rod, Bar, & Wire ASTM/ASME B/SB-691 — 45 N08367 8.2 Rod, Bar, & Wire ASTM/ASME B/SB-704 — 43 N06625 43 Welded Tube ASTM/ASME B/SB-704 — 45 N08825 45 Welded Tube ASTM/ASME B/SB-705 — 43 N06625 43 Welded Pipe ASTM/ASME B/SB-705 — 45 N08825 45 Welded Pipe ASTM/ASME B/SB-709 — 45 N08028 45 Plate, Sheet, & Strip ASTM/ASME B/SB-710 — 46 N08330 45 Welded Pipe ASTM/ASME B/SB-710 — 46 N08332 45 Welded Pipe ASTM B718 — 45 N06333 43 Plate, Sheet, & Strip ASTM B719 — 45 N06333 43 Bar ASTM B720 — 45 N08310 — Seamless Tube ASTM B722 — 45 N06333 43 Seamless Pipe & Tube ASTM B723 — 45 N06333 43 Welded Pipe ASTM B725 — 41 N02200 41 Welded Pipe ASTM B726 — 45 N06333 43 Welded Tube ASTM/ASME B/SB-729 — 45 N08020 45 Seamless Pipe & Tube ASTM B755 — 43 N06110 43 Plate, Sheet, & Strip
(Continued)
79 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM B756 — 43 N06110 43 Rod & Bar ASTM B756 — 43 N06110 43 Rod & Bar ASTM B757 — 43 N06110 43 Welded Pipe ASTM B758 — 43 N06110 43 Welded Tube ASTM B759 — 43 N06110 43 Seamless Pipe & Tube ASTM/ASME B/SB-804 — 45 N08367 8.2 Welded Pipe ASTM/ASME B/SB-804 — 45 N08367 8.2 Welded Pipe ASTM A813 N08367 45 N08367 8.2 Welded Pipe ASTM A813 N08367 45 N08367 8.2 Welded Pipe ASTM B814 — 45 N06920 43 Plate, Sheet, & Strip ASTM A814 N08367 45 N08367 8.2 Cold Worked Welded Pipe ASTM A814 N08367 45 N08367 8.2 Cold Worked Welded Pipe ASTM/ASME B/SB-815 — 49 R31233 — Rod ASTM/ASME B/SB-818 — 49 R31233 — Plate, Sheet, & Strip ASTM/ASME B/SB-861 1 51 R50250 51 Seamless Pipe ASTM/ASME B/SB-861 11 51 R52250 51 Seamless Pipe ASTM/ASME B/SB-861 12 52 R53400 52 Seamless Pipe ASTM/ASME B/SB-861 13 51 R53413 52 Seamless Pipe ASTM/ASME B/SB-861 14 52 R53414 52 Seamless Pipe ASTM/ASME B/SB-861 15 52 R53415 52 Seamless Pipe ASTM/ASME B/SB-861 16 51 R52402 51 Seamless Pipe ASTM/ASME B/SB-861 16H 51 R52402 51 Seamless Pipe ASTM/ASME B/SB-861 17 51 R52252 51 Seamless Pipe ASTM/ASME B/SB-861 18 53 R56322 53 Seamless Pipe ASTM/ASME B/SB-861 19 53 R58640 54 Seamless Pipe ASTM/ASME B/SB-861 2 51 R50400 51 Seamless Pipe ASTM/ASME B/SB-861 20 53 R58645 54 Seamless Pipe ASTM/ASME B/SB-861 21 53 R58210 54 Seamless Pipe ASTM/ASME B/SB-861 23 54 R56407 53 Seamless Pipe ASTM/ASME B/SB-861 24 54 R56405 53 Seamless Pipe ASTM/ASME B/SB-861 25 54 R56403 53 Seamless Pipe ASTM/ASME B/SB-861 26 51 R52404 51 Seamless Pipe ASTM/ASME B/SB-861 26H 51 R52404 51 Seamless Pipe ASTM/ASME B/SB-861 28 53 R56323 53 Seamless Pipe ASTM/ASME B/SB-861 29 54 R56404 53 Seamless Pipe ASTM/ASME B/SB-861 2H 51 R50400 51 Seamless Pipe ASTM/ASME B/SB-861 3 52 R50550 52 Seamless Pipe ASTM/ASME B/SB-861 33 51 R53442 54 Seamless Pipe ASTM/ASME B/SB-861 34 52 R53445 54 Seamless Pipe ASTM/ASME B/SB-861 35 54 R56340 53 Seamless Pipe ASTM/ASME B/SB-861 5 54 R56400 53 Seamless Pipe ASTM/ASME B/SB-861 7 51 R52400 51 Seamless Pipe ASTM/ASME B/SB-861 7H 51 R52400 51 Seamless Pipe ASTM/ASME B/SB-861 9 53 R56320 53 Seamless Pipe
(Continued)
80 AWS B2.1/B2.1M-BMG:2014
Table C.1 (Continued) List of Base Metal Specifications—Nonferrous Alloys
Base Metal Type, Grade, or Material UNS ISO 15608 Standard Specification Alloy Designation Number Number Group Product Form ASTM/ASME B/SB-862 1 51 R50250 51 Welded Pipe ASTM/ASME B/SB-862 11 51 R52250 51 Welded Pipe ASTM/ASME B/SB-862 12 52 R53400 52 Welded Pipe ASTM/ASME B/SB-862 13 51 R53413 52 Welded Pipe ASTM/ASME B/SB-862 14 52 R53414 52 Welded Pipe ASTM/ASME B/SB-862 15 52 R53415 52 Welded Pipe ASTM/ASME B/SB-862 16 51 R52402 51 Welded Pipe ASTM/ASME B/SB-862 16H 51 R52402 51 Welded Pipe ASTM/ASME B/SB-862 17 51 R52252 51 Welded Pipe ASTM/ASME B/SB-862 18 53 R56322 53 Welded Pipe ASTM/ASME B/SB-862 19 53 R58640 54 Welded Pipe ASTM/ASME B/SB-862 2 51 R50400 51 Welded Pipe ASTM/ASME B/SB-862 20 53 R58645 54 Welded Pipe ASTM/ASME B/SB-862 21 53 R58210 54 Welded Pipe ASTM/ASME B/SB-862 23 54 R56407 53 Welded Pipe ASTM/ASME B/SB-862 24 54 R56405 53 Welded Pipe ASTM/ASME B/SB-862 25 54 R56403 53 Welded Pipe ASTM/ASME B/SB-862 26 51 R52404 51 Welded Pipe ASTM/ASME B/SB-862 26H 51 R52404 51 Welded Pipe ASTM/ASME B/SB-862 27 51 R52254 51 Welded Pipe ASTM/ASME B/SB-862 28 53 R56323 53 Welded Pipe ASTM/ASME B/SB-862 29 54 R56404 53 Welded Pipe ASTM/ASME B/SB-862 2H 51 R50400 51 Welded Pipe ASTM/ASME B/SB-862 3 52 R50550 52 Welded Pipe ASTM/ASME B/SB-862 33 51 R53442 54 Welded Pipe ASTM/ASME B/SB-862 34 52 R53445 54 Welded Pipe ASTM/ASME B/SB-862 35 54 R56340 53 Welded Pipe ASTM/ASME B/SB-862 5 54 R56400 53 Welded Pipe ASTM/ASME B/SB-862 7 51 R52400 51 Welded Pipe ASTM/ASME B/SB-862 7H 51 R52400 51 Welded Pipe ASTM/ASME B/SB-862 9 53 R56320 53 Welded Pipe ASTM/ASME B/SB-928 5083 25 A95083 22.4 Plate & Sheet ASTM/ASME B/SB-928 5086 25 A95086 22.4 Plate & Sheet ASTM/ASME B/SB-928 5456 25 A95456 22.4 Plate & Sheet ASTM/ASME B/SB-956 — 34 C70600 34 Finned Welded Tube ASTM/ASME B/SB-956 — 34 C71500 34 Finned Welded Tube ISO 209 6082, T4, T6 23 A96082 23.1 Bar, Rod, Shapes, & Tube ISO 209 7020, T5 27 A97020 23.2 Bar, Rod, Shapes, & Tube NACE MR 01-75 100 45 N06950 43 Pipe NACE MR 01-75 110 45 N06950 43 Pipe NACE MR 01-75 125 45 N06950 43 Pipe NACE MR 01-75 140 45 N06950 43 Pipe
(Continued)
81 AWS B2.1/B2.1M-BMG:2014 Nominal Composition amless & Welded Pipe amless & Welded Pipe amless & Welded C-Mn C-Mn Pipe amless & Welded Pipe amless & Welded Pipe amless & Welded Pipe amless & Welded C-Mn Pipe amless & Welded C-Mn C-Mn C-Mn C-Mn Seamless & Welded Pipe Seamless & Welded C-Mn Seamless & Wld. Pipe & Tube& Seamless & Wld. Pipe Tube& Seamless & Wld. Pipe C-Mn C-Mn 40 [380/275]40 Sheet & Strip C Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form .2 in [mm] in Thickness or Diameter or Diameter Limitations, (Continued) Table C SteelAlloys and Steel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 1 11.11 11 1.1 1 AAR1 1.1 1 ASTM1 1.2 11 1.1 1 ABS M2011 1.1 A1018 1 ABS1 1.2 1 ABS1 ABS 1.1 1 ABS A SS 401 ABS 1.2 1 ABS1 ABS 1.2 1 ABS1 ABS 1.2 1 — ABS A — AH321 ABS 1.2 1 ABS1 ABS 1.2 1 B API K11846 K023001 ABS 1.2 1 D API DH321 ABS 1.2 1 API K021021 1.1 1 E API 2H K11846 K02101 EH321 1.1 2MT1 1 API FH321 1.1 1 API 2W K11846 55/ K018011 1.1 60/30 [415/205] 1 API 2Y K11846 421 1.1 50[440/315] 64/46 1[400/235] 58/34 API 2Y 11.11 1 API 5L 501 1.1 1[400/235] 58/34 API & Shapes Plate, Bar, 5L & Shapes Plate, Bar, 42 —1 1.1 API —[440/315] 64/46 Castings 1[400/235] 58/34 5L 501 1.1 1 API 5L & Shapes Plate, Bar, —1 1.1 A[440/315] 64/46 1 API[400/235] 58/34 & Shapes Plate, Bar, 5L & Shapes Plate, Bar, A25 Cl. I A25, — 1.1 C-Mn-Si 5L 1[440/315] 64/46 API Cl. II A25, — 1.1 1 C API 5L & Shapes Plate, Bar, & Shapes Plate, Bar, — 1.1 — API C-Mn-Si 5L A25P — & Shapes Plate, Bar, — 1.1 C-Mn-Si C API 5L B C-Si API 62/42 [425/290] 65/50 [450/345] 5L BM — C-Mn-Si API 5L BMO C-Si 65/50 [450/345] C-Mn-Si 5L BMS — 62/42 [425/290] 5L — BN — 65/50 [450/345] 5L BNO Plate Plate — 45/25 [310/170] 49/30 [340/205] BNS 45/25 [310/175] 45/25 [310/170] — Plate BQ — Se BQO Se Plate — 45/25 [310/175] Plate — —[415/240] 60/35 60/35 [415/240] C-Mn C-Mn 60/35 [415/240]Pipe Seamless & Welded 60/35 [415/240] C-Mn C-Mn 60/35 [415/240] Pipe Welded 60/35 [415/240] Pipe Welded C-Mn C-Mn 60/35 [415/240] Se Pipe Welded Se 60/35 [415/240] Se 60/35 [415/240] Se Se C-Mn C-Mn C-Mn Material Number
82 AWS B2.1/B2.1M-BMG:2014 Nominal Composition amless & Welded Pipe amless & Welded Pipe amless & Welded C-Mn C-Mn Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded C-Mn Pipe Seamless & Welded C-Mn Pipe Seamless & Welded C-Mn Pipe Seamless & Welded C-Mn C-Mn C-Mn C-Mn Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded C-Mn Pipe Seamless & Welded C-Mn Pipe Seamless & Welded C-Mn C-Mn C-Mn C-Mn Pipe Seamless & Welded Pipe Seamless & Welded C-Mn C-Mn Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 1 1.1 API 5L BQS — 60/35 [415/240] Se 111 11 11 1.1 1 11.11 11 1.2 1 API1 1.2 API 11 1.2 1 API1 1.2 1 API 5L1 1.2 5L 1 API1 1.2 1 API 5L1 1.2 1 API 5L BR1 1.2 1 API X42 5L1 1.2 1 API X42M 5L1 1.2 X42MO 1 API 5L — 11.11 1 — X42MS API 5L —1 1.2 1 API — X42N 5L1 1.2 API 1 X42NO 5L —1 1.2 1 X42NS API 5L1 1.2 — 1 API X42Q 5L —1 1.2 5L 1 X42QO API —1 1.2 1 X42QS API 5L1 1.2 — 1 60/35 [415/240] API 5L X42R —[415/290] 60/42 1 1.2 1 60/42 [415/290] API X46 5L — 60/42 [415/290]1 Se 1.2 1Pipe API Seamless & Welded X46M 5L 11.1 60/42 [415/290]1 — X46MO 1 API 5L1 1.2 1 — X46MS API 60/42 [415/290] 5L Pipe Welded — 60/42 [415/290] 1.2 API 1 Pipe Welded — X46N 5L C-Mn 1.2 60/42 [415/290] 1 X46NO API Pipe Welded 5L — 1.2 X46NS API 60/42 [415/290] 5L 60/42 [415/290] 1.2 — 5L API X46Q — 60/42 [415/290] X46QO API 5L — C-Mn X46QS API C-Mn 60/42 [415/290] 5L — X52 5L — C-Mn [435/315] 63/46 63/46 [435/315] X52M 5L — 63/46 [435/315] X52MOPipe Seamless & Welded 5L 63/46 [435/315] — X52MS — — 63/46 [435/315] X52N Pipe Welded 63/46 [435/315] X52NO Pipe Welded — C-Mn 63/46 [435/315] Pipe Welded — 63/46 [435/315] — 63/46 [435/315] 63/46 [435/315] C-Mn C-Mn [460/360] 67/52 67/52 [460/360] C-Mn 67/52 [460/360]Pipe Seamless & Welded 67/52 [460/360] 67/52 [460/360] Pipe Welded 67/52 [460/360] Pipe Welded C-Mn Pipe Welded C-Mn C-Mn C-Mn Material Number
83 AWS B2.1/B2.1M-BMG:2014 Nominal Composition t, & Strip C-Mn t, & Stript, & Strip C-Mn C-Mn eet, & Stripeet, & Strip C C eet, & Stripeet, & Stripeet, & Stripeet, & Strip C C C C ate, Sheet, & Strip C-Mn-Cr-Ni-Cu Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded C-Mn C-Mn C-Mn C-Mn 300] Plate, Sheet, & Strip C-Mn 300] Plate, Sheet, & Strip C-Mn 350] Plate, Sheet, & Strip C-Mn 380] Plate, Sheet, & Strip C-Mn 380] Plate, Sheet, & Strip C-Mn 200] Plate, Sheet, & Strip C 400/300] Plate, Shee 280/170] Plate, Sh 440/300] Plate, Shee 300/200] Plate, Sh 300/200]400/300] Plate, Sh Plate, Shee 350/250] Plate, Sh 350/250]380/250] Plate, Sh Plate, Sh Minimum Minimum Tensile/Yield 5/40.5 [410/280] Plate C-Mn Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 11 1 1 1.1 1.2 AS/NZS AS/NZS 1594 1594 HU250 HU300 — — 51/36 [ [ 58/43.5 111 11 1 1.2 1 1.2 1 AS/NZS1 2.1 AS/NZS1 1.1 AS/NZS 15941 1 AS/NZS 15941 1 15941 1.2 HA300/1 1 15941 1.4 1 HA350 AS/NZS1 1.2 1 — HA400 AS/NZS1 2.1 1 HA4N AS/NZS — 1594 1.1 1 AS/NZS — 1594 1.2 1 AS/NZS 1594 1.2 — HU300/1 AS/NZS 1594 1.1 HW350 AS/NZS 3678 — XF300 AS/NZS 3678 62.5/43.5 [430/ XF400 — 3678 3679.1 200 — 62.5/51 [430/ — 250 67/55 [460/ 250L15 40.5/25 [ 250 — — — 62.5/43.5 [430/ — 65/50 [450/340] [ 64/43.5 67/55 [460/ Pl 43.5/29 [300/200] 59. 59.5/40.5 [410/280] 59.5/38 [410/260] Plate Plate Bar & Sections C-Mn C-Mn C-Mn 1 1 1.2 API 5L X52NS — 67/52 [460/360] 111 11 11 1.2 11 1.2 11 1.2 1 API 11.11 1 API1 1.2 1 API1 1.2 API 1 5L1 1.2 1 AS 5L1 1.2 1 AS 5L 5LS1 1.1 1 AS X52Q1 1.1 1 X52QO 1548 AS AS/NZS 1.1 1 X52QS 1548 AS/NZS 1.1 X46 — 1 1548 — AS/NZS 1594 1.1 7-430 1548 — AS/NZS 1594 1.2 7-460 AS/NZS — 1594 PT430 AS/NZS — HA1 1594 PT460 HA200 — 1594 HA250 — 1594 HA250/1 — — — 67/52 [460/360] HA3 — 67/52 [460/360] — HA300 67/52 [460/360] 63/46 [435/315] — 62.5/43.5 [430/300] — 66.5/44 [460/305] 62.5/43.5 [430/300] Pipe Spiral Welded 66.5/44 [460/305] 48/29 [330/ 43.5/29 [ Plate 51/36 [ 55/36 [ Plate Plate C-Mn 43.5/29 [ [ 58/43.5 Plate C C C C Material Number
84 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Pipe C-Mn-Si ss Pipe C-Si less Pipe C less Pipe C-Mn Shapes, Bar, & RivetsShapes, Bar, C-Mn-Si Shapes, Bar, & Rivets Shapes, Bar, C-Mn-Si e, Shapes, Bar, & Rivetse, Shapes, Bar, C 415/240] Pipe Resistance Welded C-Mn [330/205] Pipe Resistance Welded C [415/240] Seamless 30 [330/205] Seamle Minimum Minimum Tensile/Yield 48/30 [330/205] Seam 58/36 [400/250] Plates60/35 [415/240] C-Mn-Si Seam 58/36 [400/250] Plates C-Mn-Si 58/36 [400/250] Plates C-Mn-Si Strength, ksi [MPa] Product Form 4 1.5 40] 2.5 65] ≤ 100] ≤ 20] 58/36 [400/250] Plates C-Mn-Si ≤ ≤ ≤ ≤ ≤ [>100] 58/36 [400/250] Plates C-Mn-Si in [mm] in 0.75 [ Thickness ≤ or Diameter or Diameter Limitations, .2 (Continued) [>20 and [>20 and [>40 and [>40 and [>65 and (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 1 11.11 1 ASTM/ASME 1.1 1 A/SA-36 11.1 ASTM/ASME 1 ASTM/ASME A/SA-53 11.1 A/SA-53 ASTM/ASME 1.1 — A/SA-53 ASTM/ASME A E, A/SA-53 B E, K02600 K02504 F K03005 A S, K03005 K02504 58/36 [400/250] 48/30 60/35 [ 48/30 [330/205] Shapes Pipe Welded Furnace C-Mn-Si C 1 1 1.1 ASTM/ASME A/SA-361 1 — 11.1 ASTM/ASME K02599 A/SA-53 B S, K03005 1 1 1.1 ASTM/ASME A/SA-106 A K02501 48/ 1 1 1.1 ASTM/ASME A/SA-36 — K02598 >0.75 and 1 1 11.1 ASTM/ASME A/SA-1061 B 1 1.1 K03006 ASTM A131 60/35 CS — 58/34 [400/235] Plate, 111 11 11 1.1 1 1.1 1 ASTM 1.1 1 ASTM 1.1 ASTM 1.1 A108 ASTM A108 ASTM A108 CW 1015 A131 CW 1018 G10150 A131 CW 1020 G10180 G10200 A B — — [–/–] –/– [–/–] –/– [–/–] –/– 58/34 [400/235] Bar 58/34 [400/235] Bar Plat Bar Plate, C C C 111 11 11 1.1 11 1.1 1 AS/NZS 11.11 1 AS/NZS 11.11 1 ASTM 3679.1 1.1 1 ASTM 3679.1 11.1 1 ASTM/ASME 11.1 ASTM 250L0 A27 A/SA-31 ASTM/ASME 11.1 250L15 A27 A/SA-36 ASTM/ASME A/SA-36 A27 — 60-30 B — 65-35 — J03000 U-60-30 — K03100 J03001 J03000 — K02595 >4 59.5/38 [410/260] 59.5/38 [410/260] 60/30 [415/205] 58/29 [400/200] Bar & Sections 65/35 [450/240] Bar & Sections 60/30 [415/205] 58/36 [400/250] Castings Rivets Castings Castings C-Mn C-Mn Bar C C C C C-Mn-Si 11 1 11.1 1 ASTM/ASME A/SA-36 11.1 ASTM/ASME A/SA-36 — — K02596 >2.5 and K02597 >1.5 and Material Number
85 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Shapes, Bar, & RivetsShapes, Bar, C-Mn-Si Shapes, Bar, & Rivets Shapes, Bar, C-Mn-Si [415/205]Flange & Fittings Pipe C-Si 26 [325/180] Seamless Tube C-Si Minimum Minimum Tensile/Yield 47/26 [325/180]60/37 [415/255] Seamless Tube Seamless Tube C C-Si Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number C K02801 55/30 [380/205] Pipe Welded C or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 1 1.1 ASTM A131111 1 D1 11 1.1 1 ASTM/ASME1 1.1 1 A/SA-134 — 11.1 ASTM/ASME1 1 A/SA-135 ASTM/ASME1 1.1 1 A/SA-135 SA36 11.11 1 11.1 ASTM1 A 1 K02599 ASTM B 11.11 1 ASTM 11.11 1 A139 K02509 ASTM A139 — K03018 1 ASTM A139 1.1 58/34 [400/235] 1 11.1 ASTM/ASME A139 ASTM Plate, A A/SA-178 ASTM/ASME A139 1.1 B A/SA-178 ASTM/ASME 58/36 [400/250] C A161 A/SA-179 K02508 A D K03003 C 48/30 [330/205] Carbon Low E K03004 60/35 [415/240] — K01504 K01200 Pipe Welded K03010 K03503 K03012 K01200 Pipe E.R.W. Pipe E.R.W. 48/30 [330/205] 60/35 [415/240] 60/42 [415/290] C [325/180] 47/26 47/26 [325/180] 60/46 [415/315] 60/37 [415/255] Pipe Welded 66/52 [455/360] C Pipe Welded C Pipe Welded Tube E.R.W. Pipe Welded Tube Tube E.R.W. Pipe Welded C C C C C C C C 111 11 11 1.1 11 1.1 1 ASTM/ASME ASTM1 1.1 1 A/SA-134 ASTM/ASME1 1.1 1 A/SA-134 11.1 ASTM/ASME A SA283, 1 A131 A/SA-134 ASTM/ASME SA283, B 1.1 1 K01400 A/SA-134 ASTM/ASME SA283, C 1.1 K01702 A/SA-134 D SA283, 11.1 ASTM/ASME K02401 DS A/SA-134 ASTM/ASME K02702 A SA285, A/SA-134 SA285, B K01700 SA285, K02200 — 45/24 [310/165][345/185] 50/27 [380/205] 55/30 60/33 [415/230] Pipe Welded 45/24 [310/165]1 Pipe Welded [345/185] 50/27 1 Pipe Welded 58/34 [400/235] Pipe1 Welded 11 Plate, 1 Pipe Welded 11.11 1 Pipe Welded ASTM/ASME1 1.1 C 1 A/SA-181 11.1 ASTM/ASME1 C 1 A/SA-192 ASTM/ASME1 1.1 C Cl. 60 1 A/SA-210 C 1.1 1 K03502 ASTM — 1.1 C 1 A-1 ASTM 1.1 C ASTM/ASME ASTM 1.1 K01201 A211 A/SA-214 K02707 ASTM/ASME A211 A/SA-216 A211 A570-30 — A570-33 WCA K02502 A570-40 60/30 K02502 K01807 J02502 K02502 47/ 49/30 [340/205] 52/33 [360/230] 47/26 [325/180] 60/30 [415/205] 55/40 [380/275] Pipe Welded Pipe Welded Tube E.R.W. Pipe Welded Castings C C C C C-Si Material Number
86 AWS B2.1/B2.1M-BMG:2014 Nominal Composition 240]Pipe Seamless & Welded C-Mn-Si 380/205]Pipe Seamless & Welded C-Mn 35 [415/240] Piping Fittings C-Mn-Si Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C K12202 66/52 [455/360] Forgings C-Mn-Si-V Number BC K01702 K02401BC K02200 K02801 50/27 [345/185] 55/30 [380/205] 50/27 [345/185] Plate 55/30 [380/205] Plate Plate Plate C C C C A K01400DA K02702 K01700 45/24 [310/165] 60/33 [415/230] 45/24 [310/165] Plate Plate Plate C C C or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 1 11.11 1 ASTM/ASME1 1.1 1 A/SA-352 ASTM/ASME1 1.1 1 A/SA-3521 1.1 1 LCA ASTM/ASME ASTM1 1.1 1 A/SA-369 LCB 11.1 ASTM/ASME1 1 J02504 ASTM/ASME A/SA-369 11.1 1 A/SA-372 A366 FPA J03003 11.1 1 ASTM FPB 11.1 ASTM K02501 A 11.1 CS ASTM K03006 A381 ASTM A381 K03002 A381 60/30 [415/205] — Y35 A381 65/35 [450/240] Y42 Y46 48/30 [330/205] — Y48 Castings 60/35 [415/240] — Castings — 60/35 [415/240] — Pipe Forged 43/20 [295/140] Pipe Forged Forgings C-Si 60/35 [415/240] C-Si 60/42 [415/290] Sheet C-Si C-Mn-Si 63/46 [435/315] 62/48 [425/330] Pipe Welded Pipe Welded C-Si Pipe Welded Pipe Welded C C C C C 11 1 11 1.1 ASTM/ASME1 1.1 A/SA-283 ASTM/ASME1 1 A/SA-283 1 1 11.11 1 ASTM/ASME 11.11 1 A/SA-285 ASTM/ASME 11.11 1 A/SA-333 ASTM/ASME 11.1 1 A/SA-333 ASTM/ASME 11.1 1 A/SA-334 ASTM/ASME 1 11.1 A/SA-334 ASTM/ASME 6 1.2 A/SA-350 1 ASTM/ASME K03008 A/SA-350 6 K03006 LF1 Cl.1 LF6, K03008 K03006 K03009 55/30 [ 60/35 [415/ 55/30 [380/205] 60/35 [415/240] 60/30 [415/205] Tube Welded Tube Welded Forgings C-Mn C-Mn-Si C-Mn-Si 1 111 1.1 ASTM/ASME 1 A/SA-283 1 1.1 ASTM/ASME 1.1 A/SA-285 ASTM/ASME A/SA-285 111 11 11 — 1 — 1 — ASTM 1 11.1 ASTM ASTM/ASME 1.1 ASTM A/SA-266 A252 ASTM/ASME A252 A/SA-283 A252 1 1 2 K03506 3 — — — 60/30 [415/205] 50/30 [345/205] 60/35 [415/240] Forgings 66/45 [455/310] Piles Pipe Piles Pipe Piles Pipe C-Si C C C 11 1 1 1.1 11.1 ASTM/ASME ASTM A/SA-234 WPB A226 K03006 — K01201 60/ 47/26 [325/180] Tube E.R.W. C-Si Material Number
87 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Seamless & Welded TubeSeamless & Welded TubeSeamless & Welded TubeSeamless & Welded C TubeSeamless & Welded C C C Minimum Minimum Tensile/Yield 60/35 [415/240] Piping Fittings C-Mn-Si Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 1 11.11 11 1.2 1 ASTM 11.11 1 11.1 ASTM1 1 ASTM A5001 1.2 1 ASTM1 1.1 1 A500 ASTM A5001 1.1 1 ASTM A5011 1.1 1 B ASTM1 1.1 1 A501 C ASTM1 — D 1 A512 K03000 ASTM1 1.1 A 1 A512 K027051 — ASTM 1 A512 B K03000 ASTM1 1.1 1008 1 A512 K030001 1010 — ASTM 1 A512 11.1 K03000 ASTM1 G10080 1012 1 A5121 G10100 1015 — ASTM 1 A512 ASTM1 G10120 — 1 58/42 [400/290] 1016 A512 G10150 1018 — ASTM 1 A512 62/46 [425/315] A512 1.1 ASTM 58/36 [400/250] 1 G10160 1019 1.1 G10180 1020 ASTM 58/36 [400/250] Tube Seamless & Welded A512 ASTM 1.1 G10190 1021 A512 70/50 [485/345] 40/20 [275/140] 1026 ASTM G10200 A512 40/20 [275/140] ASTM G10210 Tube 1110 Seamless & Welded A512 40/20 [275/140] G10260 C 1115 A512 40/20 [275/140] G11100 1117 A512 MT 1010 40/20 [275/140] G11150 Tube MT 1015 43/25 [295/170] G10100 C G11170 Tube MT 1020 G10150 43/25 [295/170] Tube 50/30 [345/205] G10200 Tube 50/30 [345/205] 55/35 [380/240] Tube Tube 55/35 [380/240] Tube 55/35 [380/240] C Tube 40/20 [275/140] 40/20 [275/140] C Tube 43/25 [295/170] Tube C 50/30 [345/205] C Tube C Tube C Tube Tube Tube C C Tube C C C C C C C C 111 11 1 11.11 11 1.1 1 ASTM ASTM/ASME1 1.1 1 A/SA-414 ASTM/ASME 1.1 1 A/SA-414 ASTM/ASME A381 1.1 1 A/SA-414 11.1 ASTM/ASME A A/SA-414 ASTM/ASME 11.1 B A/SA-414 ASTM/ASME Y50 C A/SA-420 K01501 D K02201 E WPL6 K02503 — K02505 K03006 K02704 45/25 [310/170] 50/30 [345/205] 55/33 [380/230] 64/50 [440/345] 60/35 [415/240] 65/38 [450/260] Sheet Sheet Pipe Welded Sheet Sheet Sheet C C C C C-Mn C-Mn 1 1 11.1 ASTM A500 A K03000 45/33 [310/230] Material Number
88 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form 25] 60/32 [415/220] Plate C ≤ 1 [>25]1 [ 60/32 [415/220] Plate C-Si in [mm] in ≤ Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 0210002403 60/32 [415/220] 65/35 [450/240] Plate Plate C-Mn-Si C-Mn-Si UNS Table C K02800K01800 65/35 [450/240] 55/30 [380/205] Plate Plate C-Si C-Si Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 1 1 1.1 1 ASTM/ASME 1.1 A/SA-516 1.1 ASTM ASTM 65 A519 K A519 1008 1012 G10080 G10120 40/20 [275/140] 40/20 [275/140] Tube Tube C C 111 11 11 1.1 11 1.1 1 ASTM1 1.1 1 ASTM/ASME ASTM1 1.1 1 A/SA-513 ASTM/ASME1 1.1 1 A512 A/SA-513 ASTM/ASME1 1.1 1 A512 A/SA-513 10081 — 1 MTX 1015 1010 ASTM1 1.1 ASTM/ASME 1 MTX 1020 G10080 1015 A/SA-513 ASTM/ASME1 — — 1 A/SA-513 G101001 1.1 — ASTM/ASME 1 A513 G10150 A/SA-513 1017 ASTM/ASME1 1.1 1 A/SA-513 1018 ASTM/ASME1 1.1 1 CW 1015 A/SA-513 G10170 1019 ASTM/ASME1 — 1 A/SA-513 G10180 1020 G101501 ASTM/ASME — 1 1021 A/SA-513 G10190 11.11 ASTM/ASME 1 42/30 [290/205] ASTM/ASME G10200 1022 A/SA-5131 1.1 1 A/SA-513 45/32 [310/220] 40/20 [275/140] G10210 1023 ASTM/ASME1 1.1 1 48/35 [330/240] 50/30 [345/205] A/SA-513 G10220 1024 ASTM/ASME1 1.1 1 1026 A/SA-513 G10230 ASTM/ASME MT 1010 — 1 48/35 [330/240] A/SA-513 G10240 Tube MT 1015 ASTM/ASME — 1 48/35 [330/240] G10260 G10100 A/SA-513 Tube1 1.1 Tube MT 1020 ASTM/ASME [–/–] –/– G10150 48/35 [330/240] A/SA-513 Tube 11.1 MTX 10151 Tube 52/38 [360/260] G10200 ASTM/ASME ASTM MTX 1020 1 A/SA-515 54/40 [370/275] — Tube 1 52/38 [360/260] Tube — 1.1 A515 52/38 [360/260] 60 ASTM/ASME Tube 1.1 52/38 [360/260] A/SA-516 C Tube 62/45 [425/310] ASTM/ASME Tube 45/32 [310/220] A/SA-516 C Tube C 55 C — Tube C 55 –/– [–/–] Tube 60 –/– [–/–] K02001 C Tube > Tube C Tube –/– [–/–] K C –/– [–/–] C C C Tube C Tube C 55/30 [380/205] C Tube C C Tube C Plate C C C C-Si 11 1 1 1.1 11.1 ASTM/ASME A/SA-515 ASTM/ASME A/SA-515 60 65 K02401 Material Number
89 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Pipe C-Mn-Si Pipe C-Mn-Si [415/240] Seamless 30 [380/205] Seamless Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 1 1.1 ASTM/ASME A/SA-524 II K02104 55/ 111 11 11 1.1 11 — 1 ASTM1 — 11 1.1 ASTM 11 1.1 ASTM 1 A519 ASTM1 — 1 A519 ASTM1 1.1 1 A5191 1.1 1015 ASTM 1 A519 ASTM1 — 1 1016 A519 ASTM1 1.1 G10150 1 1017 A5191 1.1 1018 ASTM 1 G10160 A519 1018 HR ASTM1 1.1 1 G10170 A519 G10180 ASTM1 G10180 — 1 1019 A519 11.1 ASTM1 1020 1 A519 1020 HR1 1.1 ASTM 1 G10190 A519 ASTM G102001 1.1 G10200 1 1021 A519 40/20 [275/140] ASTM1 1.1 1022 1 A519 1022 HR 40/20 [275/140] ASTM A5191 — 1 G10210 1025 HR 40/20 [275/140] G10220 ASTM1 G10220 — 1 A519 43/25 [295/170] G102501 — ASTM 1026 HR 1 1026 A519 [–/–] –/– — ASTM 1 Tube A519 MT 1010 G10260 50/30 [345/205] 1.1 ASTM 1 G10260 Tube MT 1015 A519 48/28 [330/195] G10100 11.1 –/32 [–/220] ASTM Tube MT 1020 A519 G10150 ASTM 1.1 Tube MTX 1015 A521 ASTM G10200 50/30 [345/205] ASTM/ASME MTX 1020 A521 A/SA-524 50/30 [345/205] Tube — A523 Tube [–/–] –/– A523 –/35 [–/240] Tube — CC C Tube I CC1 55/35 [380/240] C [–/–] –/– Tube 40/20 [275/140] A C B Tube — 43/25 [295/170] K02104 C — 50/30 [345/205] K02504 Tube Tube K03005 C C Tube 40/20 [275/140] C Tube 50/30 [345/205] Tube C Tube Tube C C 60/35 60/30 [415/205] Tube 66/33 [455/230] 48/30 [330/205] C C Tube 60/35 [415/240] C C Die Forging C C Die Forging C Pipe Pipe C C C C C-Mn C-Mn 111 11 1 — 1 — 1 11.1 ASTM — ASTM ASTM A526 ASTM A527 A529 A539 II II 42 — — K02703 — K01506[415/290] 60/42 42/25 [290/170] 42/25 [290/170] 45/35 [310/240] & Shapes Plate, Bar, Sheet Galvanized Sheet Galvanized Coiled Tube C-Mn C Material Number
90 AWS B2.1/B2.1M-BMG:2014 Nominal Composition [415/290][450/345] Plate & Shapes Plate & Shapes C-Mn-Si C-Mn-Si Minimum Minimum Tensile/Yield 47/26 [325/180]60/37 [415/255] Seamless Tube Seamless Tube C C-Si Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 11224 55/30 [380/205] Plate C-Mn-Ti UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 1 1.1 ASTM/ASME A/SA-556 A2 K01807 111 11 1 11.11 1 ASTM/ASME1 1.1 1 A/SA-556 11.1 ASTM/ASME1 1 A/SA-557 ASTM/ASME1 1.1 1 A/SA-557 B2 ASTM/ASME1 1.1 1 A/SA-562 A21 1.1 1 B2 K02707 ASTM1 1.1 1 ASTM1 — 1.1 K01807 1 K03007 ASTM1 1.2 1 A569 ASTM1 1.2 1 K A569 ASTM1 1.1 1 A569 ASTM1 1.1 1 A569 30 ASTM1 1.1 1 A569 33 ASTM1 1.1 1 A569 36 K02502 47/26 [325/180] ASTM1 1.2 1 A570 40 60/37 [415/255] K02502 ASTM1 1.2 1 A570 45 K02502 ASTM1 1.3 1 A570 50 K02502 ASTM1 1.2 Tube 1 E.R.W. A570 30 K02502 Tube ASTM/ASME E.R.W. ASTM1 1.2 1 A570 33 A/SA-572 K02502 11.1 ASTM/ASME1 1 A570 36 A/SA-572 K02502 11.11 1 A570[340/205] 49/30 40 ASTM K025021 42 1.1 1[360/230] 52/33 45 ASTM K025021 50 1.1 1[365/250] 53/36 50 K02502 C ASTM A5731 1.1 1[380/275] 55/40 55 C K02502 Sheet & Strip ASTM A573 1.1 — 1[415/310] 60/45 K02502 Sheet & Strip ASTM 1.1 — 1 A575[450/345] 65/50 K02502 Sheet & Strip 11.1 ASTM 58 A575[340/205] 49/30 Sheet & Strip 11.1 ASTM 65 A575[360/230] 52/33 ASTM Sheet & Strip M1008 A575[365/250] 53/36 ASTM Sheet & Strip M1010 — A575 C [380/275] 55/40 Sheet & Strip M1012 A575 — — C [415/310] 60/45 Sheet & Strip M1015 A575 — C [450/345] 65/50 60/42 Sheet & Strip M1017 — C [485/380] 70/55 M1020 65/50 Sheet & Strip — C M1023 Sheet & Strip — C Sheet & Strip — C Sheet & Strip — C 58/32 [400/220] C 65/35 [450/240] C [–/–] –/– C [–/–] –/– C [–/–] –/– Plate C [–/–] –/– Plate [–/–] –/– [–/–] –/– [–/–] –/– Bar Bar Bar Bar C Bar C Bar Bar C C C C C C C Material Number
91 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Minimum Minimum Tensile/Yield 65/46 [450/315] Plate & Shapes Mn-Cb Strength, ksi [MPa] Product Form 4 ≤ 102] ≤ in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) [>64 and (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 1 11.11 11 1.1 1 ASTM1 1.1 1 ASTM1 1.1 1 ASTM A5751 1.1 1 ASTM1 1.1 1 A576 ASTM1 1.1 1 A576 M1025 ASTM1 1.1 1 A576 G10080 ASTM1 1.1 1 A576 G10100 — ASTM1 1.1 1 A576 G10120 11.1 — ASTM1 1 A576 G10150 11.1 — ASTM1 1 A576 ASTM G10160 11.1 —1 1 A576 ASTM G10170 11.1 —1 1 A576 ASTM G10180 — A5761 1.1 1 ASTM G10190 ASTM/ASME — A5761 1.1 1 A/SA-587 G10200 ASTM/ASME — A5761 — 1 G10210 A/SA-587 — A5761 ASTM/ASME — 1 [–/–] –/– G10220 A/SA-587 —1 — — 1 G10230 [–/–] –/– — A21 — ASTM 1 G10250 [–/–] –/– —1 — B2 ASTM 1 K11500 [–/–] –/– —1 — ASTM K01807 1 [–/–] –/– A607 —1 1.1 ASTM 1 K03007 [–/–] –/– A6071 1.2 Bar ASTM 1 [–/–] –/– A611 ASTM 1.1 Bar 1 [–/–] –/– A611 45 ASTM 1.1 Bar 1 [–/–] –/– A611 50 ASTM 1.1 Bar A611 [–/–] –/– A 48/30 [330/205] ASTM 1.1 [–/–] –/– Bar A618 — B 47/26 [325/180] ASTM [–/–] –/– Bar A620 — C ASTM 60/37 [415/255] [–/–] –/– G10170 Bar A620 D [–/–] –/– C G10170 Bar A633 III Pipe E.R.W. G10170 Bar C Tube E.R.W. A633 A G10120 Bar C Tube E.R.W. B K12700 Bar C A Bar K00040 C C Bar K00040[450/310] 65/45 C [290/170] 42/25 Bar K01802[450/345] 65/50 C C [310/205] 45/30 C K12000 C [330/230] 48/33 C C >2.5 and Sheet & Strip[360/275] 52/40 Sheet & Strip C 65/50 [450/345] Sheet & Strip C Sheet & Strip 40/22 [275/150] C Sheet & Strip 40/22 [275/150] C Sheet & Strip 63/42 [435/290] C-Mn-Cb-V C C-Mn-Cb-V Tube C Sheet Plate & Shapes C Sheet C C Mn-V Mn-Cb C C Material Number
92 AWS B2.1/B2.1M-BMG:2014 Nominal Composition [415/205]Pipe Cast Centrifugal C-Si Minimum Minimum Tensile/Yield 65/46 [450/315] Plate & Shapes C-Mn-Si 60/50 [415/345]60/50 [415/345] Plate Plate C-Mn-Si-V-Cb C-Mn-Si-V-Cb 55/30 [380/205] Pipe Fusion Welded C Strength, ksi [MPa] Product Form 4 ≤ 102] 40] 70/60 [485/415] Plate C-Mn-V ≤ 50] 60/50 [415/345] Plate C-Mn-V ≤ ≤ 2 [ 1.5 [ in [mm] in ≤ Thickness ≤ or Diameter or Diameter Limitations, .2 (Continued) [>64 and (Continued) SteelAlloys and Steel 0170102203 58/40 [400/275] 65/40 [450/275] Plate Plate C-Mn-Si C-Mn-Si UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 1 1.1 ASTM A633 D K12037 >2.5 and 111 11 11 — 11 — 1 — ASTM 1 — ASTM 1 1.2 ASTM A653 ASTM/ASME 1.3 ASTM A653 A/SA-656 ASTM/ASME A653 A/SA-656 A653 33 50 37 60 40 K11804 80 — K11804 — — — 45/33 [310/230] 52/37 [360/255] 55/40 [380/275] Sheet Galvanized 82/80 [565/550] Sheet Galvanized Sheet Galvanized Sheet Galvanized 111 11 11 1.2 1 ASTM/ASME1 1.2 1 A/SA-656 ASTM/ASME1 1.1 1 A/SA-6561 — 1 T3, 50 ASTM1 — 1 T7, 501 1.1 ASTM 1 — 1 1.1 ASTM 1 A659 — ASTM1 — 1 A659 ASTM1 — 1 A659 11.11 1015 ASTM 1 A659 ASTM/ASME1 1.1 ASTM 1 A/SA-660 1016 A659 ASTM/ASME1 1.1 G10150 1 1017 A659 A/SA-662 ASTM/ASME1 1018 — 1 G10160 WCA A659 A/SA-6621 1020 — 1 G101701 G10180 — A ASTM J02504 1 10211 G10200 — B ASTM 1 10231 — ASTM 1 G10210 K A663 — ASTM 1 G10230 A663 K 1.1 ASTM 1 A663 [–/–] –/– 11.1 ASTM A663 ASTM/ASME — [–/–] –/– ASTM 1.1 A/SA-671 A663 45 [–/–] –/– 60/30 ASTM/ASME A663 A/SA-671 50 [–/–] –/– CA55 A668 55 — [–/–] –/– Sheet & Strip CB60 60 — [–/–] –/– K02801 Sheet & Strip 65 — [–/–] –/– Sheet & Strip K02401 B — Sheet & Strip — Sheet & Strip — G10200 Sheet & Strip C Sheet & Strip C C 45/25 [310/175] [–/–] –/– C 60/32 [415/220] 50/28 [345/195] C 55/30 [380/205] C 60/33 [415/230] Bars & Shapes Pipe Fusion Welded 60/30 [415/205] C 65/36 [450/250] Bars & Shapes Bars & Shapes Bar Bars & Shapes Bars & Shapes Forgings C C C C C C C C Material Number
93 AWS B2.1/B2.1M-BMG:2014 Nominal Composition [415/220] Pipe Fusion Welded C-Mn-Si [415/220] Pipe Fusion Welded C-Mn-Si 30 [380/205] Pipe Fusion Welded C Minimum Minimum Tensile/Yield 55/30 [380/205] Pipe Fusion Welded C Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number 35 K03504 60/35 [415/240] Bar C or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 1 11.1 1 ASTM/ASME 1.1 1 A/SA-671 ASTM/ASME 1.1 A/SA-671 11.1 ASTM/ASME CB65 A/SA-671 ASTM/ASME A/SA-671 CC60 K02800 CC65 CE55 K02100 K02403 K02202 65/35 [450/240] 60/32 [415/220] 65/35 [450/240] Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded C-Si C-Mn-Si C-Mn-Si 111 11 1 11.11 1 ASTM/ASME1 1.1 1 A/SA-671 ASTM/ASME1 1.1 1 A/SA-672 11.1 ASTM/ASME1 1 CE60 A/SA-672 ASTM/ASME1 1.1 1 A/SA-672 A45 ASTM/ASME1 1.1 K02402 1 A/SA-672 A50 11.1 ASTM/ASME1 1 A55 A/SA-672 ASTM/ASME K017001 1.1 1 A/SA-672 B55 K02200 ASTM/ASME1 1.1 1 K02801 A/SA-672 B60 ASTM/ASME1 1.1 1 B65 A/SA-672 K02001 11.1 ASTM/ASME1 1 A/SA-672 ASTM/ASME C55 K02401 11.11 1 A/SA-672 K02800 ASTM/ASME 60/32 C60 11.11 1 A/SA-672 ASTM/ASME C65 K01800 11.11 1 A/SA-675 45/24 [310/165] E55 ASTM/ASME K02100 11.11 1 A/SA-675 50/27 [345/185] E60 ASTM/ASME K02403 11.11 55/30 [380/205] 1 A/SA-675 K02202 ASTM/ASME 45 11.1 Pipe Fusion Welded 1 1 A/SA-675 55/30 [380/205] K02402 ASTM/ASME 50 11.1 Pipe Fusion Welded 1 1 A/SA-675 60/32 [415/220] Pipe Fusion Welded 55 11.11 65/35 [450/240] 1 ASTM 60 — 11.1 Pipe Fusion Welded 1 1 55/30 [380/205] ASTM 65 — 11.1 Pipe Fusion Welded 1 1 60/32 [415/220] Pipe C Fusion Welded ASTM — 11.1 A694 1 65/35 [450/240] C ASTM — 11.1 Pipe Fusion Welded A694 55/ 1 C ASTM/ASME ASTM — 11.1 Pipe Fusion Welded A694 60/32 C-Si A/SA-695 ASTM/ASME F42 Pipe Fusion Welded A694 1.2 A/SA-696 C C-Si F46 A694 B, F48 ASTM K03014 45/23 [310/160] C-Si C-Mn-Si B F50 K03014 50/25 [345/170] C-Mn-Si F52 K03014 55/27 [380/185] A707 K03014 60/30 [415/205] K03200 K03014 65/32 [450/220] L1, Cl. 1 Bar Bar K02302 60/42 [415/290] Bar 60/46 [415/315] Bar 62/48 [425/330] Bar 64/50 [440/345] 60/35 [415/240] 66/52 [455/360] Forgings Forgings C 60/42 [415/290] Forgings C Forgings C Bar Forgings C C C-Mn Forgings C-Mn C-Mn C-Mn C-Mn C-Mn-Si C-Mn Material Number
94 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Resistance Welded PipeResistance Welded PipeResistance Welded C-Mn C-Mn Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form 64] 60/42 [415/290] Plate C-Mn-Cb-V ≤ 2.5 [ in [mm] in Thickness ≤ or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 11 — 1 — 1 — ASTM 1 — ASTM 1.4 ASTM A795 ASTM A795 ASTM A795 E, B A795 A808 F S, A — S, B — — — — K11852 [415/–] 60/– [415/–] 60/– [415/–] 60/– [415/–] 60/– Pipe Welded Furnace Seamless Pipe Seamless Pipe C-Mn C-Mn 111 11 11 1.2 1 11.11 1 11.1 ASTM1 1 ASTM1 1.2 1 ASTM1 1.2 1 A707 ASTM A7071 — 1 ASTM A7071 — 1 L1, Cl. 21 — ASTM 1 L2, Cl. 1 A707 K023021 — ASTM 1 L2, Cl. 2 A707 K03301 11.11 ASTM 1 A707 L3, Cl. 1 K033011 1.2 ASTM 1 A707 L3, Cl. 2 ASTM K12510 1.2 1 A707 L4, Cl. 1 11.1 K12510 ASTM 1 A707 ASTM/ASME L4, Cl. 2 11.1 ASTM A709 K12089 A/SA-727 ASTM/ASME L5, Cl. 1 — K12089 A/SA-765 A709 66/52 [455/360] L5, Cl. 2 K20934 60/42 [415/290] A709 — 36 K20934 ASTM 66/52 [455/360] I 50 60/42 [415/290] K02506 50S A795 66/52 [455/360] Forgings — Forgings K03046 60/42 [415/290] Forgings — 66/52 [455/360] — E, A Forgings 60/42 [415/290] Forgings 66/52 [455/360] Forgings — C-Mn 60/36 [415/250] Forgings C-Mn Forgings C-Mn 60/30 [415/205][400/250] 58/36 C-Mn-V-N Forgings 1.8Ni-0.6Mn-0.3Mo C-Mn-V-N [450/345] 65/50 1.8Ni-0.6Mn-0.3Mo [450/345] 65/50 Forgings 1.1.2Cu-1Ni-0.7Cr-0.5Mn & Shapes Plate, Bar, 1.2Cu-1Ni-0.7Cr-0.5Mn Forgings & Shapes Plate, Bar, & Shapes Plate, Bar, [415/–] 60/– C-Mn C-Mn-Si C-Mn C-Mn C-Mn-Si 111 11 11 1.1 11 1.1 1 ASTM1 1.1 1 ASTM1 1.1 1 ASTM1 1.1 1 A830 ASTM 1.1 1 A830 ASTM 1.1 1 A830 ASTM 1.1 1006 A830 ASTM 1.1 1008 A830 ASTM G10060 1009 A830 ASTM G10080 1010 A830 G10090 1012 A830 G10100 1015 A830 G10120 1016 G10150 1017 G10160 1018 40/20 [275/140] G10170 40/20 [275/140] G10180 40/20 [275/140] 40/20 [275/140] 40/20 [275/140] Plate 40/20 [275/140] Plate 40/20 [275/140] Plate 40/20 [275/140] Plate 43/25 [295/170] Plate Plate Plate C Plate C Plate C C C C C C C Material Number
95 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number CS, A —[275/140] 40/20 Sheet C or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 11 1.1 11 1.1 1 ASTM1 1.1 1 ASTM1 1.1 1 11.1 ASTM1 1 A830 ASTM1 1.1 1 A830 ASTM ASTM/ASME1 1.1 1 A830 A/SA-8361 1.1 1019 1 A830 ASTM A8301 1.1 1020 1 ASTM1 1.1 — G10190 1021 1 ASTM1 1.2 G10200 1022 1 A857 1023 ASTM1 1.2 G10210 1 A857 ASTM1 1.2 G10220 — 1 A857 G10230 ASTM1 1.2 1 A857 25 ASTM1 1.3 1 A935 30 ASTM1 1.1 1 A935 33 43/25 [295/170] ASTM1 1.1 1 A935 36 — 43/25 [295/170]1 Cl. 45 ASTM1 1.2 1 A935 — 43/25 [295/170]2 Cl. 45 ASTM1 1.1 1 A935 — 43/25 [295/170]1 Cl. 50 ASTM/ASME — ASTM1 1.1 1 43/25 [295/170] A984 A/SA-1008 55/25 [380/175] —2 Cl. 50 ASTM/ASME —1 1.1 1 Plate A992 A/SA-10082 Cl. 55 —1 1.1 1 Plate A992 — ASTM1 1.1 CS, B 1 Plate 35 ASTM/ASME ASTM —1 1.2 1 Plate A/SA-1008 — Forgings[260/170] Plate 38/25 1 1.2 A1008 1 — —[340/205] 49/30 ASTM 1.2 A1008 DS, B 1 —[360/230] 52/33 ASTM 1.2 1[415/310] 60/45 — CS, C[365/250] 53/36 ASTM 1.3 C A1008 Sheet & Strip[380/310] 55/45 — DS, A — ASTM 1.2 C 1 Cl. HSLAS 45 A1008 Sheet & Strip[450/345] 65/50 C-Si-Ti ASTM C 2 Cl. HSLAS 45 A1008 — — Sheet & Strip[415/345] 60/50 Sheet & Strip ASTM C —1 Cl. HSLAS 50 A1008 — Sheet & Strip[450/380] 65/55 C Sheet & Strip2 Cl. HSLAS 50 A1008 — Sheet & Strip2 Cl. HSLAS 55 40/20 [275/140] A1008 — Sheet & Strip C 60/35 [415/240] — HSLAS-F 50 Sheet & Strip C-Mn-Cb-V C 65/50 [450/345] C-Mn-Cb-V C 65/50 [450/345] 40/22 [275/150] — C-Mn-Cb-V C 40/20 [275/140][415/310] 60/45 Sheet C-Mn-Cb-V 40/22 [275/150] Pipe[380/310] 55/45 C-Mn-Cb-V Plate & Shapes Shapes[450/345] 65/50 Sheet[415/345] 60/50 [450/380] 65/55 Sheet Sheet Sheet Sheet[415/345] 60/50 C-Mn Sheet C C-Mn-Si Sheet C Sheet C Sheet C C C C C C C C Material Number
96 AWS B2.1/B2.1M-BMG:2014 Nominal Composition 30 [340/205]30 [360/230]33 Sheet & Strip[380/275]40 Sheet & Strip[450/345]50 Sheet & Strip C C Sheet & Strip C C Minimum Minimum Tensile/Yield 53/36 [365/250]53/36 [365/250]53/36 [415/310]60/45 Sheet & Strip[415/310]60/45 Sheet & Strip Sheet & Strip Sheet & Strip C C C C Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number B —[275/205] 40/30 Sheet & Strip C B —[275/205] 40/30 Sheet & Strip C or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 11 1.1 11 1.1 1 ASTM1 1.1 1 ASTM1 1.1 1 ASTM1 1.2 A1011 1 ASTM1 1.2 A1011 1 ASTM 1.2 A1011 1 SS 33 ASTM 1.2 A1011 1 SS 36, 1 ASTM 1.2 A1011 SS 36, 2 ASTM 1.2 A1011 — — SS 40 ASTM A1011 SS 45, 1 — ASTM A1018 SS 45, 21 Cl. HSLAS 45 A1018 — — SS 502 Cl. HSLAS 45 A1018 — — 1 Cl. HSLAS 50 — — — 52/ 55/ [415/310] 60/45 [380/310] 55/45 65/ [450/345] 65/50 Sheet & Strip Sheet & Strip Sheet & Strip C C C 111 11 11 1.1 11 1.1 1 ASTM1 1.1 1 ASTM1 1.1 1 ASTM1 1.1 A1008 1 ASTM1 1.1 A1008 1 ASTM1 1.1 A1008 1 SS 25 ASTM1 1.1 A1008 1 SS 30 ASTM/ASME ASTM1 1.1 A1008 1 SS 33, 1 A/SA-10111 1.1 A1008 1 — SS 33, 2 ASTM1 1.1 A1011 CS, 1 — SS 40, 1 — ASTM1 1.1 1 SS 40, 2 — ASTM/ASME ASTM1 1.2 A1011 1 A/SA-1011 — CS, A1 1.2 A1011 1 — ASTM1 1.2 A1011 DS, 1 CS, C ASTM 1.2 — 1 CS, D ASTM 1.3 A1011 1 DS, A 42/25 [290/170] ASTM 1.21 Cl. HSLAS 45 A1011 — 45/30 [310/205] 48/33 [330/230] ASTM 1.12 Cl. HSLAS 45 — A1011 — 48/33 [330/230] ASTM —1 Cl. HSLAS 50 A1011 — 52/40 [360/275] ASTM2 Cl. HSLAS 50 A1011 — 52/40 [360/275] Sheet2 Cl. HSLAS 55 A1011 — Sheet A1011 — Sheet[275/205] 40/30 HSLAS-F 50 Sheet — Sheet 40/30 [275/205] SS 30 Sheet[275/205] 40/30 [415/310] 60/45 Sheet & Strip 40/30 [275/205][380/310] 55/45 —[450/345] 65/50 C Sheet & Strip[415/345] 60/50 C Sheet & Strip Sheet & Strip C [450/380] 65/55 Sheet & Strip Sheet & Strip C Sheet & Strip C C [415/345] 60/50 Sheet & Strip C Sheet & Strip C C 49/ C Sheet & Strip C C C C C C Material Number
97 AWS B2.1/B2.1M-BMG:2014 Nominal Composition e, Bar, & Shapese, Bar, & Shapese, Bar, C-Mn-Si-Cb-V C-Mn-Si-Cb-V Seamless & Welded FittingsSeamless & Welded FittingsSeamless & Welded FittingsSeamless & Welded C-Mn C-Mn C-Mn [330/205][415/240][415/290] Fittings Fittings Fittings C-Mn-Si C-Mn-Si C-Mn-Si 30 [340/205]30 [360/230]33 Sheet & Strip Sheet & Strip C C Minimum Minimum Tensile/Yield 53/36 [365/250]53/36 [400/250]58/36 Sheet & Strip Sheet & Strip C C Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 11 11 1.2 11 1.2 11 1.2 1 CSA 11.11 1 CSA 11.11 1 CSA G40.21 11.1 CSA1 1 G40.21 11.1 CSA1 1 G40.21 11.1 CSA 300W1 1 Z245.1 300WT 11.1 CSA1 1 Z245.1 11.1 CSA 350W1 1 Z245.1 — 11.1 CSA1 172 — 1 Z245.1 11.1 CSA1 207 Z245.11 1 — 11.1 CSA1 241 Z245.11 1 11.1 CSA —1 290 Z245.11 2 207 11.1 MSS —1 Z245.12 2 241 11.1 MSS —1 Z245.12 2 290 MSS — 1.2 2 SP-75 — 248 AAR[450/305] 65/44 1.3 2 SP-75 65/44 [450/305] — 290 1.2 ABS WPHY-42 SP-75 —[450/345] 65/50 1.3 ABS & Shapes Plate, Bar, WPHY-46 M201 — Plat ABS — 45/25 [310/170] WPHY-52 — ABS ABS — & Shapes 48/30 [330/205] Plate, Bar, ABS — 60/35 [415/240] B ABS 60/42 [415/290] C-Mn AH36 48/30 ABS AH40 Pipe 60/35 C-Mn K11852 DH36 — Pipe 60/42 K11857 DH40 Pipe 60/36 [415/250] K11852 60/42 [415/290] Pipe 60/42 [415/290] K11857 63/46 [435/315] 66/52 [455/360] Flanges C [490/350] 71/51 Flanges C [510/395] 70/38 [485/260] 74/57 C [490/350] 71/51 & Shapes Plate, Bar, C [510/395] 74/57 & Shapes Plate, Bar, & Shapes Plate, Bar, C-Mn-Si Castings & Shapes Plate, Bar, C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si C-Mn-Si 111 11 11 1.1 1 1.1 1 ASTM 1.1 1 ASTM 1.1 ASTM 1.1 A1018 A1018 CSA A1018 CSA SS 33 SS 36, 1 G40.21 SS 36, 2 G40.21 — — 260W — 260WT — — 52/ [415/260] 60/38 60/38 [415/260] & Shapes Plate, Bar, Plat C-Mn 111 11 1 1.2 1 1.3 1 ASTM 1.2 ASTM 1.1 ASTM A1018 ASTM2 Cl. HSLAS 50 A10182 Cl. HSLAS 55 A1018 — A1018 — HSLAS-F 50 — SS 30 —[415/345] 60/50 [450/380] 65/55 [415/345] 60/50 Sheet & Strip Sheet & Strip 49/ Sheet & Strip C C C Material Number
98 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded C-Mn C-Mn C-Mn C-Mn Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded C-Mn C-Mn C-Mn C-Mn Pipe Seamless & Welded C-Mn Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 21 21 1.2 21 1.3 21 1.2 2 ABS1 1.3 2 ABS1 1.2 2 ABS1 ABS 1.3 2 ABS1 ABS 1.2 2 API1 ABS 1.3 2 API EH36 11.11 ABS 2 API EH40 2.1 2 API 2H K11852 FH36 2.1 API 2 2W K11857 FH40 2.1 API 2Y K11852 1.3 API 2Y K11857 50 5L API 60 API 5L 50T 5L 60 —[490/350] 71/51 X56 5L —[510/395] 74/57 X56M 5L — X56MO[490/350] 71/51 & Shapes Plate, Bar, — —[510/395] 74/57 X56MS & Shapes Plate, Bar, — — X56N & Shapes Plate, Bar, — & Shapes Plate, Bar, C-Mn-Si — C-Mn-Si 70/50 [485/345] 75/60 [515/415] C-Mn-Si 70/50 [485/345] C-Mn-Si 75/60 [515/415][490/385] 71/56 71/56 [490/385] 71/56 [490/385] PlatePipe Seamless & Welded Plate 71/56 [490/385] Plate 71/56 [490/385] Pipe Welded Plate Pipe Welded C-Mn Pipe Welded C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn C-Mn 111 21 21 3.1 21 3.1 21 3.1 2 API 11.11 2 API1 2.1 2 API1 2.1 API 2 5L1 2.1 2 API 5L1 1.3 2 API 5L1 3.1 5L 2 API X56Q1 3.1 2 X56QO API 5L1 3.1 2 X56QS API 5L 11.11 — 2 API X60 5L — 2.1 2 API X60M 5L — 2.1 API X60MO 2 5L 2.1 — X60MS API 5L — 3.1 API — X60N 5L 5L API X60Q — X60QO API 5L — X60QS 71/56 [490/385] 5L 71/56 [490/385] — X65 5L — 71/56 [490/385] X65M 5L — X65MO[515/415] 75/60 — X65MS 75/60 [515/415] 75/60 [515/415] —Pipe Seamless & Welded — X65Q 75/60 [515/415] — 75/60 [515/415] Pipe Welded — Pipe Welded 75/60 [515/415] C-Mn 75/60 [515/415] Pipe Welded 75/60 [515/415] [535/450] 78/65 78/65 [535/450] 78/65 [535/450] C-Mn Pipe Seamless & Welded C-Mn 78/65 [535/450] C-Mn 78/65 [535/450] Pipe Welded Pipe Welded C-Mn Pipe Welded C-Mn C-Mn C-Mn Material Number
99 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Pipe C-Mn-Si Shapes, Bar, & Rivets Shapes, Bar, C-Mn-Si Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded C-Mn C-Mn [485/275] Seamless 36 [485/250]36 Flanges & Fittings C Minimum Minimum Tensile/Yield 62.5/46 [430/320]69.5/58 [480/400] Plate75.5/65 [520/450] Plate Plate C-Mn C-Mn C-Mn Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 2 1.2 ASTM A131 AH32 — 64/46 [440/315] Plate, 1 2 3.1 API 5L X65QO — 78/65 [535/450] 111 21 21 3.1 21 1.2 21 1.3 2 API AS ASTM1 1.2 2 AS ASTM1 1.2 2 A9451 1.2 2 A945 AS 5L1 1.2 2 AS1 1.2 2 50 AS AS/NZS1 1.2 2 X65QS 65 1548 AS/NZS1 1.2 2 1548 AS/NZS 36781 1.3 2 — 1548 — AS/NZS 36781 1.3 5-490 2 — AS/NZS 36781 1.3 7-490 2 AS/NZS 3678 3001 1.3 PT490 2 300L15 AS/NZS — 36781 1.2 2 AS/NZS — 3678 3501 1.2 2 350L15 — — AS/NZS — 36781 1.2 2 AS/NZS 3678 4001 1.2 2 400L15 3679.1 — AS/NZS — 70/50 [485/345]1 1.2 78/65 [535/450] 2 3679.1 AS/NZS 78/65 [540/450] 4501 1.2 2 450L15 3679.1 — AS/NZS —1 1.3 2 300 3679.1 AS/NZS1 1.3 300L0 71/52 [490/360] 2 3679.1 — AS/NZS — 300L151 1.3 71/46 [490/320] 2 Plate 3679.1 AS/NZS 11.1 71/46 [490/320] 62.5/46 [430/320] 2 — Plate 350 — 3679.1 AS/NZS 1.1 350L0 2 — ASTM 3679.1 11.1 350L15 65/52 [450/360] 65/52 [450/360] ASTM/ASME 3679.1 Plate 11.1 ASTM A/SA-105 — 400 — ASTM/ASME Plate 400L0 A27 — A/SA-106 70/58 [485/400] Plate Plate 400L15 C-Mn-Si A27 — C-Mn-Si-Ti 75.5/65 [520/450] — — Plate C Plate 70-36 — 64/46 [440/320] 64/46 [440/320] K03504 70-40 64/46 [440/320] Plate J03501 K03501 C J02501 Plate C-Mn C 69.5/52 [480/360] 70/52 [485/360] Bar & Sections Bar & Sections C 69.5/52 [480/360] Bar & Sections C-Mn C-Mn 75.5/58 [520/400] Bar & Sections 75.5/58 [520/400] Bar & Sections Bar & Sections 75.5/58 [520/400] 70/ C-Mn C-Mn 70/36 [485/250] 70/40 C-Mn Bar & Sections C-Mn C-Mn Bar & Sections 70/40 [485/275] Bar & Sections C-Mn C-Mn C-Mn Castings Castings C-Mn C-Mn C-Mn C C Material Number
100 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Shapes, Bar, & RivetsShapes, Bar, C-Mn-Si Shapes, Bar, & Rivets Shapes, Bar, & Rivets Shapes, Bar, & Rivets Shapes, Bar, C-Mn-Si C-Mn-Si & Rivets Shapes, Bar, C-Mn-Si & Rivets Shapes, Bar, C-Mn-Si C-Mn-Si [485/250][485/275]Flange & Fittings Pipe Seamless Tube C-Si C-Mn-Si 55 [450/380] Forgings 1Ni-1Cu-0.75Cr-Mo-Nb 40 [485/275] Piping Fittings C-Mn-Si Minimum Minimum Tensile/Yield 67/46 [460/315]67/46 & Shapes Plate, Bar, C 70/40 [485/275] Castings C-Mn-Si 63/42 [435/290]63/42 & Shapes Plate, Bar, C Strength, ksi [MPa] Product Form 4 1.5 38] ≤ 100] ≤ 19][485/345] 70/50 & Shapes Plate, Bar, C ≤ ≤ ≤ in [mm] in 0.75 [ Thickness ≤ or Diameter or Diameter Limitations, .2 (Continued) [>19 and [>19 and [>38 and (Continued) SteelAlloys and Steel 02803 75/40 [515/275] Plate C-Mn-Si UNS Table C Number 3 K12202 75/60 [515/415] Forgings C-Mn-Si-V or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 2 3.3 ASTM/ASME A/SA-350 LF787, Cl. 2 K20747 65/ 111 21 2 11.11 2 ASTM/ASME 11.21 2 A/SA-266 ASTM/ASME 11.1 2 A/SA-266 ASTM/ASME 11.11 2 A/SA-266 ASTM/ASME 11.1 21 A/SA-299 ASTM/ASME 31 1.3 2 A/SA-350 4 ASTM/ASME1 2 K03506 A/SA-350 A 11.11 2 K05001 LF2 ASTM/ASME 11.1 LF6, Cl. 2 A/SA-352 K03017 11.1 K 2 K03011 ASTM/ASME ASTM 11.1 A/SA-372 LCC 11.1 ASTM A356 J02505 ASTM B 70/36 [485/250] [515/260] 75/37.5 A381 70/36 [485/250] A381 K04001 1 70/36 [485/250] Y52 Forgings Forgings Y56 J03502 Forgings — Forgings — 75/45 [515/310] C-Si C-Si C-Mn-Si 70/36 [485/250] C-Mn-Si Forgings 66/52 [455/360] 71/56 [490/385] Castings Pipe Welded C-Mn-Si Pipe Welded C-Si C C 1 2 1.2 ASTM A242 1 K11510 >0.75 and 1 2 1.2 ASTM A131 AH36 — 71/51 [490/350] Plate, 111 21 21 1.2 21 1.2 2 ASTM1 1.1 2 ASTM1 1.2 2 ASTM1 1.2 2 A131 11.1 ASTM1 2 A131 ASTM/ASME 11.1 ASTM1 2 A/SA-178 A131 ASTM/ASME 11.1 DH321 2 A/SA-181 A131 ASTM/ASME DH36 1.1 2 A/SA-210 A131 D1 ASTM/ASME 1.1 Cl. 70 2 — E A/SA-216 11.1 ASTM/ASME EH32 — A/SA-216 ASTM/ASME C K03502 EH36 2 1.2 K02709 A/SA-234 WCB — WCC — 1.2 ASTM K03501 WPC J03002 — J02503 ASTM K03501 A242 64/46 [440/315] A242 70/36 70/40 [485/275] 71/51 [490/350] Plate, 1 Plate, 70/40 64/46 [440/315] 58/34 [400/235] 70/36 [485/250] 1 71/51 [490/350] K11510 Tube E.R.W. 70/40 [485/275] Plate, Plate, 70/ Plate, >1.5 and K11510 Castings Castings C-Mn-Si C-Si C-Mn-Si Material Number
101 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Minimum Minimum Tensile/Yield 70/35 [485/240] Plate C-Mn-Si 73/37 [505/255] Plate C-Mn-Si 60/40 [415/275]60/40 Plate & Bar C-Mn-Si-Cb-V 67/46 [460/315]67/46 [435/290]63/42 Plate & Bar Plate & Bar C-Mn-Si-Cb-V C-Mn-Si-Cb-V Strength, ksi [MPa] Product Form 4 8 200] ≤ 10] 75/38 [515/260] Plate C-Mn-Si 100] 20][485/345] 70/50 Plate & Bar C-Mn-Si-Cb-V ≤ ≤ ≤ ≤ ≤ in [mm] in 0.75 [ Thickness 0.375 [ ≤ or Diameter or Diameter Limitations, ≤ .2 (Continued) [>15 and <19] [>15 [>10 and <15] [>10 [>20 and <40] [>20 [>40 and (Continued) [>100 and [>100 and SteelAlloys and Steel UNS 31200 70/40 [485/275] Castings C-Mn-Ni Low Table C K03101 70/38 [485/260] Plate C-Si Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 2 11.2 ASTM/ASME A/SA-455 — K03300 1 211 11.2 ASTM/ASME1 2 A/SA-4551 21 1.1 2 11.1 — ASTM/ASME1 2 ASTM/ASME A/SA-487 11.11 2 A/SA-508 ASTM/ASME 11.11 16, Cl. A K03300 2 A/SA-508 <0.750 and >0.580 11.11 2 J ASTM 11 1.1 2 1A ASTM 11.1 2 ASTM/ASME ASTM A512 1.2 2 A/SA-513 K13502 K13502 11.1 A512 ASTM/ASME 11.1 ASTM A/SA-513 1025 A513 ASTM/ASME 1025 A/SA-515 1030 G10250 1030 A513 CW 1020 G10250 70 G10300 G10200 G10300 CW 1025 70/36 [485/250] 70/36 [485/250] G10250 56/40 [385/275] Forgings 55/35 [380/240] Forgings 65/40 [450/275] 62/45 [425/310] [–/–] –/– [–/–] –/– Tube Tube Tube C Tube C Tube Tube C C C C C C 111 21 21 — 21 — 2 — ASTM 2 — ASTM 2 — ASTM A441 11.2 ASTM A441 ASTM/ASME ASTM A/SA-455 A441 1 Group A441 2 Group A441 — 3 Group — 4 Group — 5 Group K03300 — <0.580 and >0.375 — —[485/345] 70/50 [485/345] 70/50 [460/315] 67/46 [435/290] 63/42 [435/290] 63/42 Shapes Shapes Shapes Shapes Shapes C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Si-Cb-V C-Mn-Si-Cb-V 1 2 — ASTM A441 — K12211 11 2 2 — — ASTM ASTM A441 A441 — — K12211 >1.5 and K12211 >4 and 111 21 2 11.1 2 11.1 2 ASTM/ASME ASTM 11.1 A/SA-414 ASTM/ASME — A/SA-414 A381 F ASTM G Y60 K03102 A441 K03103 — — K12211 >0.75 and <1.5 70/42 [485/290] 75/45 [515/310] 75/60 [515/415] Sheet Sheet Pipe Welded C-Mn C-Mn C Material Number
102 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Sheet, Bar, & ShapesBar, Sheet, C-Mn-Si-Cb-V [515/415] Plate & Shapes C-Mn-Si 40 [485/275] Seamless Tube C-Mn-Si 45 [450/310]45 Sheet & Strip[450/310]45 Sheet & Strip C-Mn C-Mn Minimum Minimum Tensile/Yield 65/45 [450/310] Plate C-Mn-Si Strength, ksi [MPa] Product Form 4 ≤ 102] 64] 70/50 [485/345] Plate C-Mn-Si ≤ ≤ 2.5 [ in [mm] in Thickness ≤ or Diameter or Diameter Limitations, .2 (Continued) [>64 and (Continued) SteelAlloys and Steel 02700 70/38 [485/260] Plate C-Mn-Si UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 21 21 1.1 21 1.1 2 ASTM1 1.1 2 11.1 ASTM1 2 ASTM1 1.2 2 A519 ASTM 11.11 2 A519 ASTM1 — 2 A519 CW 1018 ASTM A519 — 2 CW 1020 G10180 11.1 ASTM 2 A519 CW 1022 G10200 11.1 A519 ASTM ASTM G10220 1025 1.2 CW 1025 A519 ASTM ASTM/ASME CW 1026 A521 A/SA-537 G10250 G10250 A529 G10260 A529 1030 Cl. 1 CE 50 G10300 [–/–] –/– K12437 [–/415] –/60 55 [–/–] –/– — — 53/30 [365/205][–/450] –/65 — [–/–] –/– Tube Tube 75/55 [515/380] Tube Tube Tube 75/37 [515/255][485/345] 70/50 Tube Tube[485/380] 70/55 C C & Shapes Plate, Bar, Die Forging & Shapes Plate, Bar, C C C C-Mn C C-Mn C C 1 2 11.1 ASTM/ASME A/SA-516 70 K 11 211 2 1.21 ASTM/ASME 2 A/SA-537 11.11 2 ASTM/ASME 11.1 2 A/SA-541 ASTM/ASME 11.1 Cl. 1 2 A/SA-541 ASTM/ASME 11.1 A/SA-556 ASTM/ASME 1 K12437 1.3 A/SA-557 1A and >2.5 C2 ASTM K03506 C2 K03020 K03006 A572 K03505 55 70/36 [485/250] 70/36 [485/250] 70/ — 70/40 [485/275] Forgings Forgings Tube E.R.W. 70/55 [485/380] C-Mn-Si C-Si Plate, C-Mn 111 21 2 11.11 2 ASTM/ASME 11.11 2 A/SA-572 11.11 2 ASTM 11.11 2 ASTM 601 1.4 2 ASTM A5731 1.4 2 ASTM A595 1.4 2 — ASTM A595 1.4 2 ASTM 1.4 70 A606 ASTM 1.4 A A606 ASTM B 2, CR, AR A606 ASTM — A606 2, HR, A K02004 — HR, AR 2, A606 K02005 A606 2, HR, N — 75/60 — 4, CR, AR 4, HR, A — — — 65/55 [450/380] 70/42 [485/290] 70/60 [485/415] 65/ 65/45 [450/310] Tube 70/50 [485/345] Welded Tube Welded 65/45 [450/310] Plate 65/ Sheet & Strip Sheet & Strip 65/45 [450/310] Sheet & Strip C Low C Low Sheet & Strip C-Mn C C-Mn C-Mn C-Mn Material Number
103 AWS B2.1/B2.1M-BMG:2014 Nominal Composition 485/275]Pipe Cast Centrifugal C-Mn-Si [485/250]Pipe Cast Centrifugal C-Si [485/260][485/345][515/275] Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded C-Mn-Si C-Mn-Si C-Mn-Si Minimum Minimum Tensile/Yield 70/60 [485/415]70/60 [485/415] Plate Plate C-Mn-Si-V-Cb C-Mn-Si-V-Cb 67/46 [460/315] Tube Mn-Cu-V 67/46 [460/315] Tube Mn-Cu-V 67/46 [460/315] Tube Mn-Cu-V Strength, ksi [MPa] Product Form 19] 70/50 [485/345] Tube Mn-Cu-V 19] 70/50 [485/345] Tube Mn-Cu-V 19] 70/50 [485/345] Tube Mn-Cu-V 64] 70/50 [485/345] Plate & Shapes Mn-Cb 64] 70/50 [485/345] Plate & Shapes C-Mn-Si ≤ ≤ ≤ 25] 80/70 [550/485] Plate C-Mn-V ≤ ≤ ≤ 1 [ 2.5 [ 2.5 [ in [mm] in ≤ 0.75 [ 0.75 [ 0.75 [ Thickness ≤ ≤ ≤ ≤ ≤ or Diameter or Diameter Limitations, .2 (Continued) [>19 and <38] [>19 [>19 and <38] [>19 [>19 and <38] [>19 (Continued) SteelAlloys and Steel 02007 70/43 [485/295] Plate C-Mn-Si UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 2 1.1 ASTM A633 C K12000 1 2 1.1 ASTM A633 D K12037 111 21 21 1.3 2 ASTM/ASME1 1.3 2 A/SA-656 ASTM/ASME1 1.3 2 A/SA-656 ASTM/ASME1 1.1 2 A/SA-656 11.1 ASTM/ASME1 70 2 T3, 60 A/SA-660 ASTM/ASME1 1.1 2 A/SA-660 T7, 60 ASTM/ASME1 — 2 K11804 WCB A/SA-662 — 1 — 2 WCC 11.1 — 1 ASTM 2 J03003 11.11 C ASTM J02505 2 ASTM 11.1 2 A663 ASTM/ASME ASTM 11.1 2 A/SA-671 A663 K ASTM/ASME A668 1.2 A/SA-671 11.1 ASTM/ASME A668 CB70 A/SA-671 ASTM/ASME 70 CC70 A/SA-671 75 K03101 C 70/36 CD70 70/40 [ K02700 D CK75 — K12437 G10250 — K02803 G10300 70/38 [485/260] 70/38 70/50 70/39 [485/270] Pipe Fusion Welded 66/33 [455/230] 75/40 75/41 [515/285] 75/37 [515/255] Bars & Shapes Bars & Shapes Forgings C-Si Forgings C C C C 1 2 1.2 ASTM A618 II K12609 1 2 1.2 ASTM A618 II K12609 >0.75 and <1.5 1 2 1.2 ASTM A618 Ib K02601 11 2 2 1.2 1.2 ASTM ASTM A618 A618 Ib Ib — K02601 >0.75 and <1.5 65/50 [450/345] Tube Seamless & Welded C-Mn 1 2 1.2 ASTM A618 Ia — >0.75 and <1.5 111 21 2 1.4 2 1.4 2 ASTM — ASTM 1.2 ASTM A606 ASTM A606 HR, AR 4, A607 A618 4, HR, N — 55 — Ia — — 70/50 [485/345] 65/45 [450/310] Sheet & Strip[485/380] 70/55 Sheet & Strip Sheet & Strip C-Mn C-Mn C-Mn-Cb-V Material Number
104 AWS B2.1/B2.1M-BMG:2014 Nominal Composition r 0.75Mn-0.6Ni-0.12P ne Piling—Plate & Ba ne Piling—Plate [485/260][515/275] Pipe Fusion Welded Pipe Fusion Welded C-Mn-Si C-Mn-Si 40 [515/275] Pipe Fusion Welded C-Mn-Si Minimum Minimum Tensile/Yield 65/45 [450/310] Pipe Fusion Welded C-Mn-Si 70/50 [485/345] Plate C-Mn-Si-Cb Strength, ksi [MPa] Product Form 40] 70/50 [485/345]64] Plate 70/50 [485/345] Pipe Fusion Welded C-Mn-Si C-Mn-Si 65] 70/50 [485/345] Plate C-Mn-Si ≤ ≤ ≤ 1.5 [ 2.5 [ 2.5 [ in [mm] in Thickness ≤ ≤ ≤ >2.5 [>65][450/310] 65/45 Plate C-Mn-Si or Diameter or Diameter Limitations, .2 (Continued) [>64 and <102] (Continued) SteelAlloys and Steel 12447 75/45 [515/310] Plate C-Mn-Si UNS Table C Number 40 K03504 70/40 [485/275] Bar C or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 11 2 2 11.1 ASTM/ASME 11.1 A/SA-672 ASTM/ASME A/SA-672 B70 C70 K03101 K02700 70/38 [485/260] 70/38 Pipe Fusion Welded C-Si 111 21 2 1.2 2 11.1 ASTM/ASME 2 A/SA-672 ASTM/ASME 11.1 A/SA-672 ASTM/ASME 1.2 A/SA-675 D701 N75 ASTM 70 K12437 2 K02803 A678 1.2 ASTM/ASME — A/SA-691 A CMSH-70 K12437 70/45 [485/310] K01600 75/40 Pipe Fusion Welded 70/35 [485/240] C-Mn-Si Bar C 111 2 2 1.4 21 11.1 ASTM/ASME1 ASTM 1.2 A/SA-6911 ASTM/ASME 2 A/SA-6911 CMS-75 2 A690 11.11 CMSH-70 2 K02803 11.11 2 K12437 ASTM 11.11 2 ASTM — >2.5 and <4 11.11 2 ASTM/ASME ASTM 11.1 A6941 2 A/SA-695 ASTM/ASME 11.1 K12249 A6941 2 A/SA-696 A6941 1.3 2 B, >4 [>100] ASTM F561 — 75/ 2 C F60 ASTM1 — 2 70/50 [485/345] F65 K03014 A7071 1.4 ASTM 2 K030141 1.4 ASTM Mari K03200 2 A707 ASTM K030141 1.4 2 L2, Cl. 3 A707 11.1 ASTM1 2 A707 L3, Cl. 3 ASTM/ASME K03301 11.1 ASTM1 2 A/SA-737 A709 ASTM/ASME L4, Cl. 3 11.1 K12510 2 A/SA-738 A709 ASTM/ASME L5, Cl. 3 11.1 K12089 2 A/SA-765 A709 68/56 [470/385]A 50W, B 1.2 K20934 75/60 [515/415] ASTMB 50W, A 70/40 [485/275] ASTM/ASME 1.250W HPS A/SA-841 77/65 [530/450] II ASTM/ASME — K12001 A/SA-841 A830 — K 75/60 [515/415]1 A, Cl. — Forgings K030471 A, Cl. 75/60 [515/415] Forgings — Bar Forgings 1025 75/60 [515/415] — 75/60 [515/415] Forgings G10250 Forgings C-Mn [485/345] 70/50 Forgings C-Mn [485/345] 70/50 [485/345] 70/50 Forgings 70/36 [485/250] C-Mn C-Mn-Si & Shapes Plate, Bar, & Shapes Plate, Bar, C-Mn & Shapes Plate, Bar, 1.8Ni-0.6Mn-0.3Mo C-Mn-V-N 1.2Cu-1Ni-0.7Cr-0.5Mn 43/25 [295/170] Forgings C-Mn C-Mn C-Mn Plate C-Mn-Si C Material Number
105 AWS B2.1/B2.1M-BMG:2014 Nominal Composition e, Bar, & Shapese, Bar, C-Mn-Si-Cb-V Plate, Bar, & ShapesPlate, Bar, & ShapesPlate, Bar, C-Mn-Si-Cb-V C-Mn-Si-Cb-V LA Plate, Bar, & ShapesLA Plate, Bar, C-Mn-P 55 [485/380]55 [515/415]60 Sheet & Strip Sheet & Strip C C Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 1 2 1.3 CSA G40.21 380W —[485/380] 70/55 & Shapes Plate, Bar, C-Mn 111 21 21 1.3 21 1.3 2 11.1 ASTM1 2 ASTM1 1.3 2 ASTM 11.11 A1011 2 ASTM1 1.3 A1018 2 ASTM A1018 1.41 Cl. HSLAS 55 2 SS 601 Cl. HSLAS 60 ASTM 1.4 A1018 2 — A1018 — 1.42 Cl. HSLAS 60 CSA1 Cl. HSLAS 65 1.2 A1018 — CSA — —2 Cl. HSLAS 65 CSA G40.21 CSA — G40.21 G40.21 350A G40.21 350AT[485/380] 70/55 350R[485/415] 70/60 — 350WT — 75/ [485/415] 70/60 [550/450] 80/65 — Sheet & Strip —[515/450] 75/65 Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip 70/50 [485/345] C 70/50 [485/345] C HSLA HSLA 70/50 [485/345] 70/50 [485/345] C C HS C Plat 111 21 21 1.2 21 1.3 2 11.1 ASTM1 2 ASTM1 1.3 2 ASTM1 1.3 2 A913 ASTM1 1.2 2 A935 ASTM A9351 1.3 2 ASTM1 1.3 2 A935 501 Cl. 55 11.1 ASTM1 21 Cl. 60 A935 ASTM1 1.3 2 A984 ASTM2 Cl. 60 —1 1.3 2 A984 — —2 Cl. 65 ASTM1 1.3 A1008 2 A1008 — ASTM1 1.31 Cl. HSLAS 55 2 501 Cl. HSLAS 60 11.1 — ASTM1 A1008 2 — 60 — ASTM 1.32 Cl. HSLAS 60 A1008 2 ASTM 1.32 Cl. HSLAS 65 A1008 2 — — ASTM 1.3 A1011 — — HSLAS-F 60 A1011 ASTM 1.31 Cl. HSLAS 55 [485/380] 70/55 1 Cl. HSLAS 60 65/50 [450/345] ASTM[515/415] 75/60 A1011 — — — ASTM2 Cl. HSLAS 60 A1011[485/415] 70/60 2 Cl. HSLAS 65 A1011 —[515/450] 75/65 [485/380] 70/55 Sheet & Strip A1011 —[515/415] 75/60 Sheet & Strip HSLAS-F 60 Shapes[485/415] 70/60 Sheet & Strip 70/50 [485/345] — SS 55[515/450] 75/65 Sheet & Strip 75/60 [515/415] C-Mn-Cb-V Sheet C-Mn-Cb-V [485/415] 70/60 [485/380] 70/55 Sheet — C-Mn-Ni-Cr-Cb-V [515/415] 75/60 C-Mn-Cb-V Sheet Pipe[485/415] 70/60 C-Mn-Cb-V Sheet Pipe[515/450] 75/65 Sheet & Strip Sheet & Strip Sheet[485/415] 70/60 Sheet & Strip C Sheet & Strip C 70/ C Sheet & Strip C C C C C C C C C Material Number
106 AWS B2.1/B2.1M-BMG:2014 Nominal Composition t, Strip C-Mn e, Bar, & Shapese, Bar, C-Mn-Si-Cb-V Plate, Bar, & ShapesPlate, Bar, & ShapesPlate, Bar, C-Mn-Si-Cb-V C-Mn-Si-Cb-V & ShapesPlate, Bar, C-Mn-Si-Cb-V LA Plate, Bar, & ShapesLA Plate, Bar, C-Mn Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded C-Mn C-Mn C-Mn Seamless & Welded FittingsSeamless & Welded FittingsSeamless & Welded FittingsSeamless & Welded C-Mn C-Mn C-Mn 450]Pipe Seamless & Welded C-Mn-Si 570/480] Plate, Shee [435/315][455/360][490/385] Fittings Fittings Fittings C-Mn-Si C-Mn-Si C-Mn-Si Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 02803 80/45 [550/310] Plate C-Mn-Si UNS Table C K12202 75/60 [515/415] Forgings C-Mn-Si-V Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 21 21 1.4 21 1.3 21 1.3 2 CSA 11.11 2 CSA 11.11 2 CSA G40.21 11.1 CSA1 2 G40.21 11.1 CSA1 2 G40.21 11.1 400AT CSA1 2 Z245.1 11.1 CSA 400W1 2 Z245.1 400WT 11.1 CSA 2 — Z245.1 11.1 CSA 317 Z245.11 2 — 11.1 CSA 359 — Z245.11 11.1 CSA 386 Z245.11 317 CSA — Z245.12 359 MSS — Z245.12 386 — Z245.12 — 317 SP-75 — 75/60 [515/415] 359 — 386 75/60 [515/415] HSLA WPHY-56 75/60 [515/415] — HS — HSLA 1 — 63/46 [435/315] —1 66/52 [455/360]1 3 71/56 [490/385] 63/46 3 11.1 66/52 3 ASTM/ASME 11.1 Pipe 71/56 A/SA-299 ASTM/ASME Pipe 63/46 [435/315] 4.1 A/SA-333 ASTM/ASME Pipe 66/52 [455/360] A/SA-350 71/56 [490/385] B 71/56 [490/385] 10 Cl.2 LF6, Flanges K Flanges C-Mn — Flanges C-Mn C-Mn C-Mn-Si C-Mn-Si C-Mn-Si 80/65 [550/ 1 2 1.3 CSA G40.21 380WT — 70/55 [485/380] Plat 1 2 1.4 CSA G40.21 400A —111 21 2 11.11 3 11.11 3 11.1 MSS1 3 11.1 MSS1 75/60 [515/415] 3 AAR1 2.2 3 SP-75 HSLA 1 2.2 API 3 SP-751 2.2 3 API WPHY-60 M201 3.1 3 API WPHY-65 3.1 5L 3 — API 3.1 — B+ API 5L 2.2 API 5L API X70 5L AS/NZS — X70M 5L X70MO 5L 1594 — X70MS 5L — — X70Q 75/60 [515/415] X70QO XF500 — 77/65 [530/450] X70QS — — — — 80/50 [550/345][570/485] 83/70 83/70 [570/485] 83/70 [570/485]Pipe Seamless & Welded Castings 83/70 [570/485] 83/70 [570/485] Pipe Welded 83/70 [570/485] [ 83/69.5 Pipe Welded C-Mn 83/70 [570/485] Pipe Welded C-Mn-Si C-Mn C-Mn C-Mn Material Number
107 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Sheet, Bar, & ShapesBar, Sheet, C-Mn-Si-Cb-V [550/415] Pipe Fusion Welded C-Mn-Si Minimum Minimum Tensile/Yield 82/48 [565/330] Forgings C 85/50 [585/345] Forgings C 80/70 [550/485]80/70 [550/485] Plate Plate C-Mn-Si-V-Cb C-Mn-Si-V-Cb 70/46 [485/315]75/50 [515/345] Plate Plate C-Mn-Si C-Mn-Si 75/55 [515/380] Plate C-Mn-Si Strength, ksi [MPa] Product Form 4 4 20 500] 250] 6 152] ≤ ≤ 10 102] 102] 20] 90/80 [620/550] Plate C-Mn-V ≤ ≤ ≤ ≤ ≤ 64] 80/55 [550/380] Plate C-Mn-Si 64] 80/60 [550/415] Plate C-Mn-Si ≤ ≤ ≤ ≤ ≤ ≤ 100] 90/55 [620/380] Forgings C ≤ 4 [ 2.5 [ 2.5 [ in [mm] in 0.75 [ ≤ >4 [>102] 70/40 [485/275] Plate C-Mn-Si Thickness ≤ ≤ ≤ or Diameter or Diameter Limitations, .2 (Continued) [>64 and [>64 and (Continued) [>250 and [>250 and [>100 and [>100 and [>102 and [>102 and SteelAlloys and Steel UNS Table C Number 7, Cl.3 K20747 75/65 [515/450] Forgings 1Ni-1Cu-0.75Cr-Mo-Nb or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 3 3 1.2 3 ASTM/ASME 1.2 A/SA-671 ASTM/ASME — A/SA-672 ASTM/ASME CD80 A/SA-675 D80 K12437 80 K12437 — 80/60 80/46 [550/315] Pipe Fusion Welded 80/40 [550/275] C-Mn-Si Bar C 1 3 11.1 ASTM A668 F — >10 and 111 31 31 2.2 3 ASTM/ASME 2.2 3 A/SA-656 ASTM/ASME — 3 A/SA-656 11.1 T3, 70 11.1 ASTM T7, 70 ASTM ASTM — A663 — A668 A668 80 F F — — — >4 and 80/44 [550/305] Bars & Shapes C 11 31 3 1.21 ASTM/ASME 3 1.2 A/SA-5371 ASTM/ASME A/SA-5371 1.2 3 ASTM/ASME Cl. 31 3 A/SA-537 Cl. 31 — 3 K12437 1 — 3 Cl. 3 K12437 — ASTM 3 — ASTM and 3 >2.5 K12437 4.1 ASTM A607 1.3 ASTM A607 ASTM/ASME ASTM A607 A/SA-656 A611 60 A633 65 80 70 — E K11804 E — — G10170 K12202[515/415] 75/60 [550/450] 80/65 [565/550] 82/80 [585/485] 85/70 80/55 [550/380] Sheet & Strip Sheet & Strip Sheet & Strip Sheet & Strip Plate & Shapes C-Mn-Cb-V C-Mn-Cb-V C-Mn-Cb-V C-Mn-Si-V C 1 3 11.1 ASTM A572 65 — 80/65 [550/450] Plate, 1 3 3.3 ASTM/ASME A/SA-350 LF78 111 3 31 11.1 3 11.1 ASTM 3 1.2 ASTM ASTM/ASME A/SA-537 1.2 A381 ASTM/ASME A513 A/SA-537 Cl. 2 Y65 CW 1026 Cl. 2 K12437 G10260 and >2.5 K12437 — [–/–] –/– 77/65 [530/450] Pipe Welded Tube C C 1 3 1.2 ASTM/ASME A/SA-537 Cl. 2 K12437 and >4 Material Number
108 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Minimum Minimum Tensile/Yield 70/46 [485/315] Plate C-Mn-Si 85/65 [585/450]75/55 [515/380] Plate Pipe Fusion Welded 80/60 [550/415]85/60 [585/415]75/55 [515/380] C-Mn-Si Plate C-Mn-Si Plate Plate C-Mn-Si-V C-Mn-Si-Cb C-Mn-Si Strength, ksi [MPa] Product Form 4 2 6 152] 50] ≤ ≤ 102] ≤ ≤ ≤ 65] 80/60 [550/415] Plate C-Mn-Si 64] 80/60 [550/415] Pipe Fusion Welded 64] C-Mn-Si 80/60 [550/415] Plate C-Mn-Si 65] 80/60 [550/415] Plate C-Mn-Si ≤ ≤ ≤ ≤ ≤ 2.5 [ 2.5 [ 2.5 [ 2.5 [ in [mm] in Thickness ≤ ≤ ≤ ≤ >2.5 [>65][515/380] 75/55 Plate C-Mn-Si or Diameter or Diameter Limitations, .2 (Continued) [>40 and [>40 and [>64 and [>64 and <102] (Continued) [>102 and [>102 and SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 11 3 3 1.1 ASTM/ASME 1.3 A/SA-765 ASTM/ASME A/SA-841 IV2 B, Cl. K02009 — 80/50 [550/345] Forgings C-Mn-Si 111 31 31 1.3 3 ASTM/ASME1 3.1 3 A/SA-8411 3.1 3 ASTM1 3.1 32 B, Cl. 11.1 ASTM1 3 11.1 ASTM1 3 A913 — ASTM1 1.3 3 A913 ASTM1 — 3 A913 11.1 ASTM A9351 3 60 11.1 A935 ASTM 3 65 ASTM 1.3 31 Cl. 65 A935 70 ASTM 1.31 Cl. 70 — A984 A1008 ASTM 1.3 — —2 Cl. 70 1 Cl. HSLAS 65 A1008 ASTM — —1 Cl. HSLAS 70 — ASTM A1008 70 — —2 Cl. HSLAS 70 A1008 A1008 — HSLAS-F 70 — — SS 80 75/60 [515/415] 80/65 [550/450][550/450] 80/65 80/70 [550/485][585/485] 85/70 —[550/450] 80/65 [585/485] 85/70 [550/485] 80/70 Shapes Sheet & Strip[550/485] 80/70 Shapes Sheet & Strip 80/70 [550/485] Shapes[550/485] 80/70 Sheet & Strip Sheet Sheet C-Mn-Ni-Cr-Cb-V C-Mn-Cb-V Sheet C-Mn-Ni-Cr-Cb-V C-Mn-Cb-V 82/80 [565/550] C-Mn-Ni-Cr-Cb-V Pipe C-Mn-Cb-V Sheet C Sheet C C C C C 1 311 1.21 ASTM/ASME 3 A/SA-6911 3 11.1 CMSH-80 31 4.1 3 K12437 ASTM 11.1 ASTM/ASME A/SA-737 ASTM/ASME 11.1 3 A/SA-738 ASTM/ASME A694 A/SA-738 11.1 C ASTM/ASME B A/SA-738 C F70 K12202 K12007 C K03014 K02008 >2.5 and K02008 82/70 [565/485] Forgings C-Mn 1 3 1.2 ASTM/ASME A/SA-691 CMSH-801 K12437 >2.5 and <4 3 11.1 ASTM/ASME A/SA-738 C K02008 >4 and 1 3 1.3 ASTM A678 B K02002 1 3 1.3 ASTM A678 C K02204 >1.5 and Material Number
109 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Plate, Bar, & ShapesPlate, Bar, & ShapesPlate, Bar, C-Mn-Si-Cb-V C-Mn-Si-Cb-V & ShapesPlate, Bar, C-Mn-Si-Cb-V LA Plate, Bar, & ShapesLA Plate, Bar, C-Mn Seamless & Welded Pipe Seamless & Welded Pipe Seamless & Welded C-Mn C-Mn Seamless & Welded FittingsSeamless & Welded C-Mn [515/415][530/450][565/485] Fittings Fittings Fittings C-Mn-Si C-Mn-Si C-Mn-Si 70 [585/485]70 Sheet & Strip C Minimum Minimum Tensile/Yield 90/80 [620/550] Plate C-Mn-Si-V-Cb Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 31 3 11.11 31 1.3 3 ASTM1 1.3 3 ASTM1 1.3 3 A1018 ASTM1 1.4 31 Cl. HSLAS 70 ASTM1 1.4 A1018 3 11.1 —12 Cl. HSLAS 70 A1018 3 CSA 11.11 A1018 3 CSA — HSLAS-F 60 11.1 CSA1 3 HSLAS-F 70 G40.21 11.1 CSA1 — 3 G40.21 11.1 CSA1 — 3 G40.21 11.1 CSA1 480A 3 G40.21 11.1 480AT CSA1 3 Z245.1 480W 11.1 CSA1 3[550/485] 80/70 Z245.1 480WT — 11.1 CSA 3 — Z245.1[550/485] 80/70 11.1 CSA 414 Z245.11 3 — — 11.1 CSA 448 Z245.11[485/415] 70/60 Sheet & Strip 11.1 CSA 483 Z245.11[550/485] 80/70 414 CSA — Sheet & Strip Z245.12 448 MSS — Z245.12 483 — Sheet & Strip Z245.12 — 414 Sheet & Strip 85/70 [585/485] SP-75 — 85/70 [585/485] 448 C HSLA — 85/70 [585/485] 483 HSLA 85/70 [585/485] WPHY-70 — C HS — HSLA — 75/60 [515/415] C — 77/65 [530/450] C 82/70 [565/485] 75/60 77/65 Pipe 82/70 Pipe 75/60 [515/415] Pipe 77/65 [530/450] 82/70 [565/485] 82/70 [565/485] Flanges Flanges C-Mn Flanges C-Mn C-Mn C-Mn-Si C-Mn-Si C-Mn-Si 111 31 3 11.11 3 11.1 3 ASTM 1.3 3 ASTM 1.3 A1011 ASTM 1.31 Cl. HSLAS 65 A1011 ASTM1 Cl. HSLAS 70 — ASTM A1011 —2 Cl. HSLAS 70 A1011 A1011 — HSLAS-F 70 — SS 70 —[550/450] 80/65 [585/485] 85/70 [550/485] 80/70 Sheet & Strip[550/485] 80/70 Sheet & Strip Sheet & Strip 85/ Sheet & Strip C C C C 111 41 4 11.11 41 2.2 4 AAR 2.2 4 3.1 4 API 3.1 API M201 2.2 API ASTM/ASME API 5L A/SA-656 5L C T3, 80 5L X80M 5L X80MO — — X80Q — X80QO — — — 90/60 [620/415] 91/80 [625/550] 91/80 [625/550] 91/80 [625/550] 91/80 [625/550] Castings Pipe Welded Pipe Welded C-Mn-Si C-Mn C-Mn Material Number
110 AWS B2.1/B2.1M-BMG:2014 Nominal Composition ate, Bar, & Shapesate, Bar, & Shapesate, Bar, C-Mn-Si C-Mn-Si Plate, Bar, & ShapesPlate, Bar, C-Mn-Si [620/550] Fittings C-Mn-Si 80 [655/550]80 Sheet & Strip C Minimum Minimum Tensile/Yield 60/30 [415/205] Seamless Tube 1Cr-V 90/70 [620/485] Plate C-Mn-Si 90/80 [620/550] Plate C-Mn-Si-V-Cb 105/70 [725/485] Plate Mn-0.5Ni-V Strength, ksi [MPa] Product Form 1.5 40] ≤ 20] 95/75 [655/515] Plate C-Mn-Si ≤ 13] 83/50 [570/345] Plate C-Mn-Si ≤ 75] 90/75 [620/515] Plate C-Mn-Si-V-N 76] 80/60 [550/415] Plate Mn-0.5Ni-V ≤ ≤ ≤ [>76] 75/55 [515/380] Plate Mn-0.5Ni-V 3 [ 3 [ 0.5 [ in [mm] in ≤ ≤ 0.75 [ Thickness ≤ ≤ or Diameter or Diameter Limitations, .2 (Continued) [>20 and [>20 and (Continued) SteelAlloys and Steel 118311203112037 90/70 [620/485] 95/75 [655/515] 90/70 [620/485] Plate Plate Plate C-Mn-Si C-Mn-Si C-Mn-Si UNS Table C Number . B J13002 90/65 [620/450] Castings Mn-V or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 111 41 41 1.3 41 — 4 ASTM1 3.1 4 ASTM/ASME1 3.1 ASTM 4 A/SA-724 ASTM/ASME1 1.1 4 A678 A/SA-724 ASTM/ASME1 — 4 A707 A/SA-7241 1.3 A 4 1.3 B ASTM 4 D L5, Cl. 4 ASTM1 1.3 C 4 K ASTM1 1.3 K20934 A984 K K12202 ASTM1 1.4 A1008 4 K ASTM1 A1011 4 HSLAS-F 80 1.3 A1011 4 CSA HSLAS-F 80 80 1.3 A1018 — 4 11.1 — CSA HSLAS-F 80 SS 80 G40.21 11.1 CSA — 90/75 [620/515] CSA — G40.21 CSA 550A — G40.21 Z245.1 550W Z245.11 — 550WT Forgings[620/550] 90/80 550 —[620/550] 90/80 550 — 1.2Cu-1Ni-0.7Cr-0.5Mn 90/80 [620/550][620/550] 90/80 — 95/ — Sheet & Strip Sheet Sheet & Strip 90/80 [620/550] Pipe[620/550] 90/80 90/80 [620/550] C & Shapes 90/80 [620/550] Plate, Bar, C Pl 90/80 C C C-Mn Pipe C-Mn 1 4 1.4 CSA G40.21 550AT — 90/80 [620/550] Pl 1 4 1.3 ASTM A678 C K02204 >0.75 and 1 4 2.2 ASTM/ASME A/SA-656 T7, 80 — 11 4 4 — 1.3 ASTM/ASME A/SA-675 ASTM 90 A678 — C K02204 90/55 [620/380] Bar C 10C10C 1 1 11.1 1.3 AAR ASTM/ASME A/SA-612 TC128 — B K02900 — 81/50 [560/345] Plate C-Mn-Si 10B 1 4.1 ASTM/ASME A/SA-213 T17 K12047 10A10A 110A 110A 4.1 110A ASTM/ASME 2.1 1 A/SA-225 ASTM/ASME 2.1 1 A/SA-225 ASTM/ASME 2.1 A/SA-225 ASTM/ASME 2.1 C A/SA-487 ASTM/ASME D A/SA-487 D 1, ACl. K12524 1, Cl K12004 J13002 K12004 >3 85/55 [585/380] Castings Mn-V Material Number
111 AWS B2.1/B2.1M-BMG:2014 Nominal Composition rip 29Cr-6.5Ni-2Mo-N rip 25Cr-5Ni-3Mo-2Cu rip 25Cr-6.5Ni-3Mo-N riprip 21Cr-3.5Ni-Mo-N 21Cr-5Mn-1.5Ni-Cu-N Strip 25Cr-7Ni-4Mo-N Strip 22Cr-5Ni-3Mo-N Strip 22Cr-5Ni-3Mo-N eet, & Strip 26Cr-4Ni-Mo Sheet, & Strip 21Cr-5Mn-1.5Ni-Cu-N e, Sheet, & Strip 29Cr-6.5Ni-2Mo-N Plate, Sheet, & St Plate, Sheet, & St 0] Plate, Sheet, & Strip 25Cr-8Ni-3Mo-W-Cu-N 0] Plate, Sheet, & St 5] Plate, Sheet, & St 485] Plate, Sheet, & Strip 26Cr-4Ni-Mo-N 550] Plate, Sheet, & 450] Plate, Sheet, & Strip 25Cr-6Ni-Mo-N 450] Plate, Sheet, & 450]450] Plate, Sheet, & Strip Plate, Sheet, & 22Cr-2Ni-Mo-N 450] Plate, Sheet, & St 650/450] Bars & Shapes 25Cr-5Ni-3Mo-2Cu 620/485] Plate, Sh 65 [690/450] Castings 25Cr-8Ni-3Mo-W-Cu-N Minimum Minimum Tensile/Yield 81/50 [560/345] Plate C-Mn-Si Strength, ksi [MPa] Product Form 6] 101/77 [700/530] Plate, 10] 109/80 [750/550] Plat ≤ ≥ 0.25 [ in [mm] in 0.40 [ Thickness ≤ ≥ or Diameter or Diameter Limitations, .2 (Continued) [>13 and <25] [>13 (Continued) 5 95/65 [655/450] Bar 22Cr-5Ni-3Mo-N 6 [<10] <0.40 116/94 [800/650] SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 10C 1 1.3 ASTM/ASME A/SA-612 — K02900 >0.5 and <1 10H10H 110H 110H 10.2 110H ASTM/ASME 10.1 1 A/SA-240 10.1 1 ASTM/ASME ASTM 10.1 S32950 A/SA-276 ASTM/ASME 10.2 A/SA-276 ASTM/ASME S32950 A276 A/SA-351 — S32205 CD3MWCuN J93380 S3220 S32550 — S32101 100/70 [690/ 100/ 94/65 [ 94/65 [650/450] Bar 21Cr-5Mn-1.5Ni-Cu-N 10H 1 10.2 ASTM/ASME A/SA-240 S32906 S3290 10H10H 110H 1 10.2 1 ASTM/ASME 10.2 A/SA-240 ASTM/ASME 10.2 A/SA-240 ASTM/ASME S32750 A/SA-240 S32760 S32750 S32906 S32760 S32906 116/80 [800/ 108/80 [745/55 10H10H 1 1 10.1 ASTM/ASME 10.2 A/SA-240 ASTM/ASME A/SA-240 S31803 S32550 S31803 S32550 90/65 [620/ 110/80 [760/55 10H10H 1 1 10.2 ASTM/ASME 10.2 A/SA-240 ASTM/ASME A/SA-240 S31200 S31260 S31200 S31260 100/65 [690/ 100/70 [690/48 10H10H 110H 1 10.1 1 ASTM/ASME 10.1 A/SA-240 ASTM/ASME 10.2 A/SA-240 ASTM/ASME A/SA-240 — 2205 329 S32202 S32205 S32900 94/65 [650/ 95/65 [655/ 90/70 [ 10H10H 1 1 10.1 ASTM/ASME 10.1 A/SA-240 ASTM/ASME A/SA-240 — — S32101 S32101 >0.25 [>6] 95/65 [655/ 10H10H 110H 110H 10.1 110H ASTM/ASME 10.2 1 A/SA-18210H ASTM/ASME 10.1 1 A/SA-18210H ASTM/ASME 10.2 1 A/SA-18210H ASTM/ASME — 10.2 1 A/SA-18210H F50 ASTM/ASME 10.1 1 A/SA-182 F51 ASTM/ASME 10.1 S32202 1 A/SA-182 F53 ASTM/ASME S31200 10.2 A/SA-182 F54 ASTM/ASME S31803 10.1 A/SA-182 F55 ASTM/ASME S32750 A/SA-240 F60 S39274 F61 S32760 S32205 — S32550 94/65 [650/450] 100/65 [690/450] S32003 90/65 [620/450] 116/80 [800/550] 116/80 [800/550] Forgings Forgings 109/80 [750/550] 95/70 [655/485] Forgings Forgings 109/80 [750/550] Forgings 90/65 [620/450] 22Cr-2Ni-Mo-N Forgings 25Cr-6Ni-Mo-N Forgings 22Cr-5Ni-3Mo-N Forgings 25Cr-7Ni-3Mo-2W-Cu-N 25Cr-7Ni-4Mo-N 25Cr-8Ni-3Mo-W-Cu-N 22Cr-5Ni-3Mo-N 25Cr-5Ni-3Mo-2Cu Material Number
112 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Tube 29Cr-6.5Ni-2Mo-N Tube 25Cr-6.5Ni-3Mo-N Tube 23Cr-4Ni-Mo-Cu-N ed Tube 26Cr-4Ni-Mo lded Tube 29Cr-6.5Ni-2Mo-N Welded TubeWelded 23Cr-4Ni-Mo-Cu-N Seamless & Welded Seamless & Welded TubeSeamless & Welded 25Cr-7Ni-3Mo-2W-Cu-N Seamless & Welded TubeSeamless & Welded 22Cr-2Ni-Mo-N 0] Tube Seamless & Welded 0] 25Cr-5Ni-3Mo-2Cu Tube Seamless & Welded 25Cr-8Ni-3Mo-W-Cu-N 0]5] Tube Seamless & Welded Bars & Shapes 21Cr-3.5Ni-Mo-N 29Cr-6.5Ni-2Mo-N 0] Seamless & Welded 485] Tube Seamless & Welded 26Cr-4Ni-Mo-N 550] Tube Seamless & Welded 25Cr-7Ni-4Mo-N 450] Tube Seamless & Welded 25Cr-6Ni-Mo-N 450]Pipe Seamless & Welded 21Cr-3.5Ni-Mo-N 440]450] Tube Seamless & Welded 485] Tube Seamless & Welded 18Cr-5Ni-3Mo-N Tube Seamless & Welded 22Cr-5Ni-3Mo-N 22Cr-5Ni-3Mo-N 450] Bars & Shapes 21Cr-5Mn-1.5Ni-Cu-N 450] Tube Seamless & Welded 21Cr-5Mn-1.5Ni-Cu-N 600/400] Seamless & Welded 620/485] Seamless & Weld [760/550][800/550] Bars & Shapes Bars & Shapes 25Cr-5Ni-3Mo-2Cu 25Cr-7Ni-4Mo-N [620/450][650/450][655/450] Bars & Shapes Bars & Shapes Bars & Shapes 22Cr-5Ni-3Mo-N 22Cr-2Ni-Mo-N 22Cr-5Ni-3Mo-N 70 [690/485] Castings 26Cr-5Ni-2Mo-3Cu Minimum Minimum Tensile/Yield 95/65 [655/450] Castings 24Cr-10Ni-4Mo-N Strength, ksi [MPa] Product Form 5] 101/77 [700/530] Tube Seamless & Welded 21Cr-5Mn-1.5Ni-Cu-N 10] 109/80 [750/550] Seamless & We ≤ ≥ 25] 100/65 [690/450] Seamless & ≤ 1 [ in [mm] in ≤ 0.40 [ 0.187 [ 0.187 Thickness ≥ ≤ or Diameter or Diameter Limitations, .2 (Continued) (Continued) 6 [<10] <0.40 116/94 [800/650] SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 10H10H 1 1 10.2 ASTM/ASME 10.2 A/SA-789 ASTM/ASME A/SA-789 S32950 S39274 S32950 S39274 100/70 [690/ 116/80 [800/550] 10H 1 10.1 ASTM/ASME A/SA-790 — S32003 90/65 [620/ 10H10H 110H 110H 10.1 110H ASTM/ASME 10.1 1 A/SA-789 ASTM/ASME 10.1 1 A/SA-789 ASTM/ASME 10.1 S31500 A/SA-789 ASTM/ASME 10.1 S31803 A/SA-789 ASTM/ASME S31500 S32205 A/SA-78910H S31803 S3230410H S32205 S32304 1 S32304 1 S32304 10.2 [>25] >1 ASTM/ASME 10.2 A/SA-789 ASTM/ASME A/SA-789 92/64 [635/ 87/58 [ S32906 90/65 [620/ S32906 95/70 [655/ S32906 S3290 10H10H 110H 110H 10.2 1 ASTM/ASME 10.2 1 A/SA-789 ASTM/ASME 10.2 A/SA-789 ASTM/ASME 10.2 S32550 A/SA-789 ASTM/ASME S32750 A/SA-789 S32550 S32760 S32750 S32900 S32760 S32900 110/80 [760/55 116/80 [800/ 109/80 [750/55 90/70 [ 10H 1 10.2 ASTM/ASME A/SA-351 CD4MCu J93370 100/ 10H10H 110H 110H 10.2 110H ASTM/ASME 10.1 1 A/SA-35110H ASTM/ASME 10.1 1 A/SA-47910H ASTM/ASME 10.1 CE8MN 1 A/SA-47910H ASTM/ASME 10.1 1 A/SA-479 J93345 10H ASTM/ASME — 10.2 1 A/SA-47910H ASTM/ASME — 10.2 1 A/SA-47910H ASTM/ASME — 10.2 S31803 1 A/SA-479 220510H 10.1 S32550 S32101 1 ASTM/ASME ASTM 10.1 S32750 S32202 1 A/SA-789 S32205 ASTM/ASME S32550 10.1 A/SA-789 ASTM/ASME S32750 10.1 A479 A/SA-789 ASTM/ASME — A/SA-789 — S32906 — 90/65 S32003 — 94/65 [650/ S32906 S32101 94/65 95/65 S32101 110/80 [>5] >0.187 S32202 116/80 [650/ 94/65 100/70 [690/48 109/80 [750/55 94/65 [650/450] 10H10H 1 1 10.2 ASTM/ASME 10.2 A/SA-789 ASTM/ASME A/SA-789 S31200 S31260 S31200 S31260 100/65 [690/ 100/65 [690/45 Material Number
113 AWS B2.1/B2.1M-BMG:2014 Nominal Composition pe 21Cr-5Mn-1.5Ni-Cu-N ed Pipe 21Cr-5Mn-1.5Ni-Cu-N lded Pipe 29Cr-6.5Ni-2Mo-N & Welded Pipe & Welded 29Cr-6.5Ni-2Mo-N 0]Pipe Seamless & Welded 25Cr-7Ni-3Mo-2W-Cu-N 0]Pipe Seamless & Welded 25Cr-8Ni-3Mo-W-Cu-N 485]Pipe Seamless & Welded 26Cr-4Ni-Mo-N 450]450]Pipe Seamless & Welded Pipe Seamless & Welded 25Cr-6Ni-Mo-N 25Cr-6.5Ni-3Mo-N 550]550]Pipe Seamless & Welded Pipe Seamless & Welded 25Cr-5Ni-3Mo-2Cu 25Cr-7Ni-4Mo-N 450]Pipe Seamless & Welded 22Cr-2Ni-Mo-N 400]Pipe Seamless & Welded 23Cr-4Ni-Mo-Cu-N 650/450]Pi Seamless & Welded 635/440]620/450]Pipe Seamless & Welded 655/450]Pipe Seamless & Welded 18Cr-5Ni-3Mo-N Pipe Seamless & Welded 22Cr-5Ni-3Mo-N 22Cr-5Ni-3Mo-N 620/485]Pipe Seamless & Welded 26Cr-4Ni-Mo [650/450] Fittings 21Cr-5Mn-1.5Ni-Cu-N 80 [760/550]80 [750/550] Fittings Fittings 25Cr-5Ni-3Mo-2Cu 25Cr-8Ni-3Mo-W-Cu-N 65 [650/450] Fittings 22Cr-2Ni-Mo-N Minimum Minimum Tensile/Yield 90/65 [620/450]95/65 [655/450] Fittings Fittings 22Cr-5Ni-3Mo-N 22Cr-5Ni-3Mo-N 116/80 [800/550] Fittings 25Cr-7Ni-4Mo-N Strength, ksi [MPa] Product Form 5][700/530] 101/77 Seamless & Weld 10][750/550] 109/80 Seamless & We ≤ ≥ in [mm] in 0.187 [ 0.187 0.40 [ Thickness ≤ ≥ or Diameter or Diameter Limitations, .2 (Continued) (Continued) 6 [<10] <0.40 116/94 [800/650] Seamless SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 10H10H 110H 110H 10.2 110H ASTM/ASME 10.2 1 A/SA-79010H ASTM/ASME 10.2 1 A/SA-79010H ASTM/ASME 10.1 S32906 1 A/SA-79010H ASTM/ASME 10.1 S32950 1 A/SA-81510H ASTM/ASME S3290 10.1 S39274 1 A/SA-81510H ASTM/ASME S32950 10.1 1 A/SA-81510H ASTM/ASME S39274 — 10.2 1 A/SA-81510H ASTM/ASME — 10.2 S31803 1 A/SA-81510H ASTM/ASME 10.2 S32205 S32101 1 A/SA-81510H ASTM/ASME S31803 10.2 S32550 S32202 1 A/SA-81510H S32205 10.2 S32750 1 S32550 ASTM 10.2 S32760 100/70 [690/ 1 S32750 ASTM 10.2 116/80 [800/55 S32760 ASTM 10.2 A890 ASTM A890 ASTM 94/65 A890 94/ A890 1A A890 1B 110/ 1C J93370 2A 109/ J93372 3A J93373 J93345 J93371 100/70 [690/485] 100/70 [690/485] 100/65 [690/450] 95/65 [655/450] Castings 95/65 [655/450] Castings Castings Castings 26Cr-5Ni-2Mo-3Cu Castings 25Cr-5Ni-3Mo-2Cu 25Cr-6Ni-3Mo-Cu-N 24Cr-10Ni-4Mo-N 25Cr-5Ni-2Mo-N 10H 1 10.1 ASTM/ASME A/SA-790 — S32101 10H10H 110H 110H 10.1 110H ASTM/ASME 10.1 1 A/SA-79010H ASTM/ASME 10.2 1 A/SA-79010H ASTM/ASME 10.2 1 A/SA-79010H ASTM/ASME — 10.1 1 A/SA-79010H ASTM/ASME — 10.1 S31200 1 A/SA-79010H ASTM/ASME 10.1 S31260 S32101 1 A/SA-79010H ASTM/ASME S31200 10.1 S31500 S32202 1 A/SA-790 [>5] >0.187 10H ASTM/ASME S31260 10.2 S31803 1 A/SA-79010H ASTM/ASME S31500 10.2 S32205 1 A/SA-790[ 94/65 ASTM/ASME S31803 10.2 S32304 1 A/SA-790 ASTM/ASME S32205 10.2 S32550 A/SA-790 ASTM/ASME S32304 10.2 S32750 A/SA-790 ASTM/ASME S32550 S32760 100/65 [690/ A/SA-790 S32750 94/65 [650/ S32900 100/65 [690/ S32760 S32906 92/64 [ S32900 90/65 [ S32906 95/65 [ 87/58 [600/ 110/80 [760/ 116/80 [800/ 109/80 [750/55 90/70 [ Material Number
114 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Strip 25Cr-4Ni-4Mo-Ti lded Tube 27Cr-1Mo lded Tube 29Cr-4Mo eet, & Strip 27Cr-1Mo-Ti Sheet, & Strip 27Cr-1Mo Sheet, & Strip 29Cr-4Mo 515] Tube Seamless & Welded 25Cr-4Ni-4Mo-Ti 515] Plate, Sheet, & 415] Tube Seamless & Welded 29Cr-4Mo-Ti 470/310] Tube Seamless & Welded 27Cr-1Mo-Ti 470/310] Plate, Sh 550/415] Plate, 550/415] Seamless & We [690/485] Castings[690/450] 25Cr-5Ni-3Mo-2Cu Castings 25Cr-8Ni-3Mo-W-Cu-N [450/275] Seamless & We [450/275]Pipe Seamless & Welded 27Cr-1Mo-Ti [450/275] Plate, 75 [690/515] Castings 25Cr-7Ni-4Mo-N 40 [485/275]40 [450/275] Tube Seamless & Welded Tube Seamless & Welded 27Cr [450/275]40 27Cr Pipe Seamless & Welded 27Cr-1Mo 65 [655/450]65 [655/450]60 [620/415] Castings Castings Castings 24Cr-10Ni-4Mo-N 25Cr-5Ni-2Mo-N 22Cr-5Ni-3Mo-N Minimum Minimum Tensile/Yield 70/55 [485/380] Bars & Shapes 29Cr-4Mo Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 10I10I 110I 110I 7.1 110I ASTM/ASME 7.1 110I A/SA-268 ASTM/ASME 7.1 110I A/SA-268 ASTM/ASME 7.1 110I 25-4-4 A/SA-268 ASTM/ASME 7.1 TP 446-1 110I A/SA-268 ASTM/ASME 7.1 TP 446-2 1 S44635 S44600 A/SA-268 TP XM-27 ASTM/ASME 7.1 1 S44600 A/SA-336 TP XM-33 ASTM/ASME 7.1 S44627 A/SA-479 FXM-27Cb ASTM/ASME 7.1 S44626 A/SA-731 S44627 ASTM/ASME XM-27 A/SA-731 TPXM-27 TPXM-33 S44627 S44627 90/75 [620/ 70/ S44626 65/ 65/40 [ 68/45 60/35 [415/240] 65/40 [450/275] 65/ 65/40 Forgings Bars & Shapes 27Cr-1Mo 27Cr-1Mo 10I10I 1 1 7.1 ASTM/ASME 7.1 A/SA-182 ASTM/ASME A/SA-240 FXM-27Cb S44627 S44635 S44635 60/35 [415/240] 90/75 [620/ Forgings 27Cr-1Mo 10I 1 7.1 ASTM/ASME A/SA-240 XM-27 S44627 65/40 10I 1 7.1 ASTM/ASME A/SA-240 XM-33 S44626 68/45 [ 10J 1 7.1 ASTM/ASME A/SA-240 S44700 S44700 80/60 [ 10J 1 7.1 ASTM/ASME A/SA-268 29-4 S44700 80/60 [ 10J10J 1 1 7.1 ASTM/ASME 7.1 A/SA-268 ASTM/ASME A/SA-479 S44735 S44700 S44735 S44700 75/60 [515/ 10H10H 110H 110H 10.1 110H 10.2 110H ASTM 10.2 110H ASTM 10.2 1 ASTM 10.1 A890 1 ASTM 10.2 A890 ASTM 10.2 A890 ASTM/ASME ASTM A928 4A A/SA-995 A928 5A A928 6A J92205 1B — J93404 2205 J93380 255 J93372 S32760 S32205 S32550 90/60 [620/415] 100/75 [690/515] 100/65 [690/450] 100/70 108/80 [745/550] 90/65 [620/450] Castings 110/80 [760/550] Castings Castings Pipe Welded Pipe Welded Pipe Welded 22Cr-5Ni-3Mo-N 25Cr-8Ni-3Mo-W-Cu-N 25Cr-7Ni-4Mo-N 25Cr-8Ni-3Mo-W-Cu-N 22Cr-5Ni-3Mo-N 25Cr-5Ni-3Mo-2Cu 10H10H 110H 110H 10.2 110H ASTM/ASME 10.2 1 A/SA-995 ASTM/ASME 10.1 1 A/SA-995 ASTM/ASME 10.2 A/SA-995 ASTM/ASME 2A 10.2 A/SA-995 ASTM/ASME 3A A/SA-995 4A J93345 5A J93371 6A J92205 J93404 J93380 95/ 95/ 90/ 100/ 100/65 Material Number
115 AWS B2.1/B2.1M-BMG:2014 Nominal Composition ed Tubeed Tube 26Cr-3Ni-3Mo 29Cr-4Mo-2Ni ee Mn-0.5Mo-0.75Ni Mn-0.5Mo-0.25Ni 450] Plate C-Mn-1Ni-1Cr-0.3Mo 450]415] Plate, Sheet, & Strip Plate, Sheet, & Strip 26Cr-3Ni-3Mo 29Cr-4Mo-2Ni 690/515]Pipe Seamless & Welded 9Ni 550/415] Seamless & Weld 585/450]550/415]Pipe Seamless & Welded Pipe Seamless & Welded 26Cr-3Ni-3Mo 29Cr-4Mo-2Ni 585/450] Seamless & Weld [725/585][795/655] Castings Castings 0.5Ni-0.5Cr-0.25Mo-V 0.5Ni-0.5Cr-0.25Mo-V [550/415]Pipe Seamless & Welded 29Cr-4Mo 80 [725/550]85 [725/585] Castings Forgings 3Ni-1.5Cr-0.5Mo 3.5Ni-1.75Cr-0.5Mo-V 55 [485/380] Bars & Shapes 29Cr-4Mo-2Ni Minimum Minimum Tensile/Yield 95/65 [655/450] Plate 5Ni-0.25Mo 100/83 [690/570]100/83 [690/570]100/83 [690/570] Plate Plat Plat Mn-0.5Mo-0.5Ni 100/75 [690/515] Piping Fittings 9Ni Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C K81340K81340 100/75 [690/515] 100/85 [690/585] Plate Plate 9Ni 9Ni Number 3 K12521 100/83 [690/570] Plate Mn-0.5Mo I K71340 100/85 [690/585] Plate 8Ni or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 10J 1 7.1 ASTM/ASME A/SA-731 S44700 S44700 80/60 11A11A 411A 411A 3.2 411A ASTM/ASME 3.1 5 A/SA-533 ASTM/ASME 3.2 5 A/SA-533 ASTM/ASME 9.23 C, Cl. A/SA-672 ASTM/ASME 3.13 Cl. D, A/SA-352 K12554 ASTM/ASME A/SA-508 J100 K12529 LC2-1 4N, Cl. 1 K12521 J42215 K22375 100/83 [690/570] 105/ 105/ Pipe Fusion Welded Mn-0.5Mo 11A 4 3.2 ASTM/ASME A/SA-5333 B, Cl. K12539 10K10K 110K 110K 7.1 110K ASTM/ASME 7.1 111A A/SA-268 ASTM/ASME 7.1 111A A/SA-479 ASTM/ASME 7.1 111A 29-4-2 A/SA-731 ASTM/ASME 7.1 1 S4480011A A/SA-731 ASTM/ASME 9.3 1 S44800 S4466011A A/SA-803 ASTM/ASME S44800 9.3 1 S4480011A A/SA-333 ASTM/ASME S44660 9.3 111A 26-3-3 A/SA-334 ASTM/ASME S44800 9.3 111A A/SA-353 ASTM/ASME 9.3 8 1 S4466011A A/SA-420 ASTM/ASME 9.3 8 111A A/SA-522 ASTM/ASME 9.3 — 111A WPL8 A/SA-522 K81340 80/60 [ ASTM/ASME 9.3 211A A/SA-553 70/ K81340 ASTM/ASME 9.3 K81340 2 I11A A/SA-553 85/65 [ 9.2 II 311A 80/60 [ ASTM/ASME ASTM 3.1 3 I A/SA-645 K81340 85/65 [585/450] 3.1 I 4 K71340 ASTM/ASME ASTM 3.1 A844 A/SA-487 ASTM/ASME 3.1 100/75 [ A A/SA-487 ASTM/ASME 100/75 [690/515] TubeB 4, Cl. Welded A734 A/SA-533E 4, Cl. — K41583 J13047 Cl. A, J13047 100/75 [690/515] Tube Welded A K81340 100/75 [690/515] 26Cr-3Ni-3Mo K21205 Forgings Forgings 105/85 9Ni 115/95 100/85 [690/585] 77/65 [530/ 9Ni 8Ni Plate 9Ni 10K10K 110K 1 7.1 1 ASTM/ASME 7.1 A/SA-240 ASTM/ASME 7.1 A/SA-240 ASTM/ASME S44660 A/SA-268 S44800 S44660 26-3-3 S44800 S44660 85/65 [585/ 80/60 [550/ 85/65 [ Material Number
116 AWS B2.1/B2.1M-BMG:2014 Nominal Composition [830/750] Plate C-Mn-1Cr.25Mo [795/690] [795/690] Forgings Forgings 3.5Ni-1.75Cr-0.5Mo-V 3.5Ni-1.75Cr-0.5Mo-V [795/690] Plate 2.75Ni-1.5Cr-0.5Mo [725/585] Forgings 3.5Ni-1.75Cr-0.5Mo-V 85 [725/585] Plate 2.75Ni-1.5Cr-0.5Mo 100 [795/690]100 Plate 3Ni-1.75Cr-0.5Mo Minimum Minimum Tensile/Yield 100/90 [690/620] Plate 1.3Ni-0.5Mo 100/90 [690/620] Plate C-Mn-Ni-Cu-V 100/90 [690/620] Plate 1.75Cr-0.5Mo-Cu 105/90 [725/620] Plate 1.75Cr-0.5Mo-Cu 105/85 [725/585] Plate 3Ni-1.75Cr-0.5Mo 110/100 [760/690]110/100 Plate 1.3Ni-0.5Mo Strength, ksi [MPa] Product Form 6 6 6 6 64] ≤ ≤ ≤ ≤ 152] 152] 152] 152] 2.5 32] [795/690] 115/100 Plate 0.5Cr-0.25Mo-Si 32] [760/690] 110/100 Plate 0.5Cr-0.25Mo-Si ≤ 38] [795/690] 115/100 Forgings 0.5Cr-0.25Mo-Si 64] [760/690] 110/100 Plate C-Mn-Ni-Cu-V 64] [760/690] 110/100 Plate 1.75Cr-0.5Mo-Cu 64] [795/690] 115/100 Plate 1.75Cr-0.5Mo-Cu 64] [795/690] 115/100 Forgings 1.75Cr-0.5Mo-Cu ≤ ≤ ≤ ≤ ≤ ≤ ≤ 50] [795/690] 115/100 50] Plate [795/690] 115/100 Plate 1.3Ni-0.5Mo 1.3Ni-0.5Mo ≤ ≤ ≤ ≤ ≤ ≤ ≤ 2 [ 2 [ 1.5 [ 2.5 [ 2.5 [ 2.5 [ 2.5 [ in [mm] in ≤ ≤ 1.25 [ 1.25 [ Thickness ≤ ≤ ≤ ≤ ≤ ≤ ≤ or Diameter or Diameter Limitations, .2 (Continued) [>50 and [>50 and [>64 and [>64 and [>64 and [>64 and (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 11B 1 3.1 ASTM/ASME A/SA-592 A K11856 11B11B 1011B 1011B 3.1 10 ASTM/ASME 3.1 10 A/SA-508 ASTM/ASME 3.1 A/SA-508 3.1 4N, Cl. 211B ASTM11B 5, Cl. 2 K22375 10 ASTM11B 10 K4236511B A514 3.1 1011B A514 3.1 1111B ASTM/ASME ASTM 3.1 11 A/SA-543 ASTM/ASME M 1.4 12 A/SA-543 M 4.2 115/100 A517 B Cl. 2 ASTM 3.1 K11683 C Cl. 2 115/100 ASTM K42339 K11683 ASTM A709 M >2.5 and — A852 A51470W HPS K11683 — — 115/ R K12043 115/100 — [585/485] 85/70 90/70 [620/485] & Shapes Plate, Bar, Plate C-Mn C-Mn 11B 12 3.1 ASTM A514 R — >2.5 and 11B 10 3.1 ASTM A514 M K11683 >2 and 11B 1 3.1 ASTM/ASME A/SA-517 A K11856 11B11B 14 2 3.1 3.1 ASTM ASTM A517 A514 C E K11511 <1.25 [<32] K21604 >2.5 and [795/690] 115/100 Plate 1.2Mn-0.2Mo 11B 2 3.1 ASTM A514 E K21604 11B 2 3.1 ASTM/ASME A/SA-517 E K21604 >2.5 and 11B11B — 1 3.1 3.1 AS/NZS ASTM 3597 A514 700PV A — K11856 120/109 11B 2 3.1 ASTM/ASME A/SA-517 E K21604 11B 2 3.1 ASTM/ASME A/SA-592 E K11695 11A 5 3.1 ASTM/ASME A/SA-508 5, Cl.1 K42365 105/85 11A11A 5 5 3.1 ASTM/ASME 3.1 A/SA-543 ASTM/ASME A/SA-543 B Cl. 1 C Cl. 1 K42339 — 105/ Material Number
117 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Minimum Minimum Tensile/Yield 100/90 [690/620] Plate 1.2Mn-0.2Mo 105/90 [725/620] Forgings 1.75Cr-0.5Mo-Cu 100/90 [690/620] Plate C-0.5Mo 105/90 [725/620] Forgings 0.75Ni-0.5Cr-0.5Mo-V 100/90 [690/620] Plate Mn-Mo-B 100/90 [690/620] Plate Mn-Mo-B Strength, ksi [MPa] Product Form 6 6 6 6 4 4 ≤ ≤ ≤ ≤ ≤ ≤ 152] 152] 152] 152] 102] 102] 32] [795/690] 115/100 Plate 0.5Cr-0.2Mo-V 32] [760/690] 110/100 Plate 0.5Cr-0.2Mo-V 32] [795/690] 115/100 Plate C-0.5Mo 64] [760/690] 110/100 Plate 1.2Mn-0.2Mo 64] [760/690] 110/100 Plate C-0.5Mo 64] [760/690] 110/100 Plate 0.75Ni-0.5Cr-0.5Mo-V 64] [795/690] 115/100 Plate 0.75Ni-0.5Cr-0.5Mo-V 64] [760/690] 110/100 Plate Mn-Mo-B 64] [795/690] 115/100 Forgings 0.75Ni-0.5Cr-0.5Mo-V 64] [760/690] 110/100 Plate Mn-Mo-B 64] [760/690] 110/100 Plate Mn-Mo-B ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ 50]50] [795/690] 115/100 [795/690] 115/100 Plate Plate Mn-Mo-B Mn-Mo-B 50] [760/690] 110/100 Plate 0.5Ni-0.5Cr-0.25Mo-V 50] [795/690] 115/100 Plate 0.5Ni-0.5Cr-0.25Mo-V ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ 2 [ 2 [ 2 [ 2 [ 2.5 [ 2.5 [ 2.5 [ 2.5 [ 2.5 [ 2.5 [ 2.5 [ 2.5 [ in [mm] in ≤ ≤ ≤ ≤ 1.25 [ 1.25 [ 1.25 [ 2.5 and 2.5 and 2.5 and 2.5 and Thickness ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ 64 and 64 and ≤ ≤ ≤ ≥ ≥ or Diameter or Diameter Limitations, ≥ ≥ .2 (Continued) [ [ [>64 and [>64 and [>64 and [>64 and (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 11B11B 411B 411B — 4 — 6 — ASTM 3.1 ASTM ASTM A782 ASTM A782 A782 A514 1 1 1 C — — K11511 — [795/690] 115/100 97/80 [670/550] 107/90 [740/620] Plate Plate Plate 1Mn-1Cr-1Si-0.5Mo-Zr 1Mn-1Cr-1Si-0.5Mo-Zr 1Mn-1Cr-1Si-0.5Mo-Zr 11B 6 3.1 ASTM A514 C K11511 >2.5 and 11B 6 3.1 ASTM A514 J K11625 11B 4 3.1 ASTM/ASME A/SA-517 B11B 6 K11630 3.1 ASTM A514 J K11625 >2.5 and 11B11B 6 6 3.1 3.1 ASTM/ASME ASTM A/SA-517 A517 S K — K11523 11B 2 3.1 ASTM/ASME A/SA-592 E K11695 11B 3 3.1 ASTM A514 F K11576 11B11B 3 3 3.1 3.1 ASTM/ASME ASTM A/SA-517 A514 F H K11576 K11646 11B 6 3.1 ASTM A514 K K11523 11B11B 311B 3 3.1 ASTM/ASME 3 3.1 A/SA-517 ASTM/ASME A/SA-592 3.1 ASTM/ASME H A/SA-592 F K11646 F K11576 K11576 11B 6 3.1 ASTM A514 K K11523 >2.5 and 11B 4 3.1 ASTM A514 B K11630 11B 6 3.1 ASTM A514 T — 11B 6 3.1 ASTM A517 J K11625 11B 6 3.1 ASTM A514 S — 11B 6 3.1 ASTM A514 T — >2.5 and Material Number
118 AWS B2.1/B2.1M-BMG:2014 Nominal Composition .25Ni-1Cr-0.5Mo .25Ni-1Cr-0.5Mo 380] Tube 0.5Ni-0.5Cr-0.2Mo 60 [585/415]60 [585/415] Seamless Tube Piping Fittings 9Cr-1Mo-V 9Cr-1Mo-V 50 [415/345]60 [515/415] Plate Plate 1Ni-1Cu-0.75Cr-Mo-Nb 1Ni-1Cu-0.75Cr-Mo-Nb Minimum Minimum Tensile/Yield 90/64 [620/440] Seamless Tube 9Cr-2W 100/90 [690/620] Plate 1 105/90 [725/620] Plate 1 100/90 [690/620] Plate 1.3Ni-1.3Cr-0.5Mo-V 105/90 [725/620] Plate 1.3Ni-1.3Cr-0.5Mo-V Strength, ksi [MPa] Product Form 6 4 6 6 ≤ ≤ ≤ ≤ 152] 102] 152] 152] 19] 90/80 [620/550] Plate 1Ni-1Cu-0.75Cr-Mo-Nb 64] [760/690] 110/100 Plate 1.25Ni-1Cr-0.5Mo 64] [795/690] 115/100 Plate 1.25Ni-1Cr-0.5Mo 64] [760/690] 110/100 Plate 1.3Ni-1.3Cr-0.5Mo-V 64] [795/690] 115/100 Plate 1.3Ni-1.3Cr-0.5Mo-V ≤ ≤ ≤ ≤ ≤ 50] [795/690] 115/100 Plate Mn-Mo-B 51] 85/75 [585/515] Plate 1Ni-1Cu-0.75Cr-Mo-Nb 51] 72/60 [495/415] Plate 1Ni-1Cu-0.75Cr-Mo-Nb ≤ ≤ ≤ ≤ ≤ ≤ ≤ 2 [ 2 [ 2 [ 2.5 [ 2.5 [ 2.5 [ 2.5 [ in [mm] in ≤ ≤ ≤ 0.75 [ Thickness ≤ ≤ ≤ ≤ ≤ or Diameter or Diameter Limitations, .2 (Continued) [>64 and [>64 and [>64 and [>64 and (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 15E15E 115E 115E 6.4 115E ASTM/ASME 6.4 115E A/SA-182 ASTM/ASME 6.4 115E A/SA-182 6.4 1 F91 ASTM/ASME ASTM 6.4 1 A/SA-213 F92 ASTM/ASME 6.4 A/SA-213 K90901 6.4 A199 T91 ASTM/ASME K92460 ASTM A/SA-234 T92 K90901 T91 A217 WP91 K92460 K90901 K90901 C12A 85/60 [585/415] 90/64 [620/440] J84090 85/ Forgings Forgings 85/ 85/60 [585/415] 85/60 [585/415] Seamless Tube 9Cr-1Mo-V 9Cr-2W Castings 9Cr-1Mo-V 9Cr-1Mo-V 11B11B 6 8 3.1 3.1 ASTM ASTM A517 A514 T P — K21650 >2.5 and 11B 8 3.1 ASTM A514 P K21650 11B 8 3.1 ASTM/ASME A/SA-517 P K21650 >2.5 and 11B 8 3.1 ASTM/ASME A/SA-517 P K21650 11B 9 3.1 ASTM A514 Q — 11B 9 3.1 ASTM A514 Q — >2.5 and 11B 9 3.1 ASTM/ASME A/SA-517 Q — 11B 9 3.1 ASTM/ASME A/SA-517 Q — and >2.5 12B12B 112C 1 3.3 1 3.3 ASTM 3.3 ASTM ASTM A710 A710 A710 A Cl. 3 A Cl. 3 K20747 A Cl. 1 K20747 K20747 >2 [>51] 75/ 11B11B 911C 911C — 1 — 1 3.3 ASTM ASTM/ASME 3.3 ASTM A/SA-859 ASTM/ASME A519 A/SA-859 A Cl. 1 A519 A Cl. 2 K20747 4130 K20747 8630 G41300 G86300 65/55 [450/380] 75/65 [515/450] 75/55 [515/380] 75/55 [515/ Forgings Forgings Tube 1Ni-1Cu-0.75Cr-Mo-Nb 1Ni-1Cu-0.75Cr-Mo-Nb 1Cr-0.2Mo 12A 1 3.3 ASTM A710 A Cl. 2 K20747 >2 [>51] 60/ 12A 1 3.3 ASTM A710 A Cl. 2 K20747 Material Number
119 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Pipe 9Cr-1Mo-V Pipe C-0.5Mo ss Pipe 9Cr-2W [415/205] Seamless Tube 0.5Cr-0.5Mo 60 [585/415] Seamless 30 [380/205]32 [415/220]28 [365/195] Seamless Tube Seamless Tube30 [380/205] Seamless Tube30 [380/205] C-0.5Mo Piping Fittings C-0.5Mo Tube E.R.W. C-0.5Mo 30 [380/205] C-0.5Mo Seamless C-0.5Mo Minimum Minimum Tensile/Yield 90/64 [620/440] Seamle 65/35 [450/240] Castings C-0.5Mo Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 11820 65/37 [450/255] Plate C-0.5Mo UNS Table C Number . 2 K90901 85/60 [585/415] Plate 9Cr-1Mo-V or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 333 13 13 1.1 1 ASTM/ASME3 1.1 1 A/SA-209 ASTM/ASME3 1.1 1 A/SA-209 ASTM/ASME3 4.2 1 A/SA-209 ASTM/ASME T13 1.1 1 A/SA-213 T1a 11.2 ASTM/ASME3 1 A/SA-217 ASTM/ASME T1b3 1.1 1 A/SA-234 K11522 ASTM/ASME K12023 T2 1.1 1 A/SA-250 WC1 K11422 ASTM/ASME 1.1 1 WP1 A/SA-250 ASTM/ASME 4.2 K11547 A/SA-250 J12524 ASTM/ASME T1 1.1 K12821 A/SA-250 T1a ASTM/ASME A/SA-335 T1b K11522 55/ K12023 T2 60/ K11422 P1 53/ K11547 60/30 K11522 55/ 55/ 60/32 [415/220] 53/28 [365/195] 60/30 [415/205] 55/ Tube E.R.W. Tube E.R.W. Tube E.R.W. C-0.5Mo C-0.5Mo 0.5Cr-0.5Mo 33 1 1 1.1 1.1 ASTM/ASME ASTM A/SA-204 A161 A T1 K K11522 55/30 [380/205] Tube C-0.5Mo 1A1A 41A 41A — 41A — 41A 1.3 ASTM 41A — ASTM 41A ASTM — 4 A615 11.1 4 CSA A615 — A706 CSA 11.1 CSA 40 G30.18 CSA 60 G30.18 CSA G30.18 60 300R — G30.18 400R G30.18 400W — — — 500R 500W — — — — 60/40 [415/275] 90/60 [620/415] 80/60 [550/415] 60/40 [415/275] 78.5/58 [540/400] 78.5/58 [540/400] Rebar [675/500] 98/72.5 90.5/72.5 [625/500] Rebar Rebar Rebar Rebar Rebar Rebar Rebar C C C C C C C C 15E 1 6.4 ASTM/ASME A/SA-691 91 K91560 85/60 [585/415] Pipe Fusion Welded 9Cr-1Mo-V 15E15E 115E 115E 6.4 115E ASTM/ASME 6.4 115E A/SA-335 ASTM/ASME 6.4 1 A/SA-336 6.4 1 P92 ASTM/ASME ASTM 6.4 A/SA-369 F91 ASTM/ASME 5.4 A/SA-369 ASTM/ASME K92460 A356 A/SA-387 FP91 K90901 FP92 91, Cl K90901 12A K92460 J84090 85/60 [585/415] 85/60 [585/415] 90/64 [620/440] Forgings 85/60 [585/415] Pipe Forged Pipe Forged Castings 9Cr-1Mo-V 9Cr-1Mo-V 9Cr-2W 9Cr-1Mo-V 15E 1 6.4 ASTM/ASME A/SA-335 P91 K90901 85/ Material Number
120 AWS B2.1/B2.1M-BMG:2014 Nominal Composition pe 1.5Si-0.5Mo Pipe 0.5Cr-0.5Mo 205]Pipe Cast Centrifugal 0.5Cr-0.5Mo 415/205] Seamless Pi 450/240]415/205]Pipe Cast Centrifugal Pipe Cast Centrifugal C-0.5Mo C-0.5Mo-Si [380/205] Seamless [380/205] Pipe Forged 0.5Cr-0.5Mo 30 [380/205] Pipe Forged C-0.5Mo Minimum Minimum Tensile/Yield 67/46 [460/315]67/46 Plate & Bar Mn-0.6Cr-0.4Cu-Si-Nb 67/46 [460/315]67/46 Plate & Bar Mn-0.4Cr-0.4Cu-Si-V 63/42 [435/290]63/42 Plate & Bar Mn-0.4Cr-0.4Cu-Si-V 67/46 [460/315]67/46 Plate & Bar Mn-0.6Cr-0.3Cu-Si-V 63/42 [435/290]63/42 Plate & Bar Mn-0.6Cr-0.3Cu-Si-V 67/46 [460/315]67/46 Plate & Bar Mn-0.5Cr-0.3Cu-Si-V 63/42 [435/290]63/42 Plate & Bar Mn-0.5Cr-0.3Cu-Si-V 65/35 [450/240] Castings C-0.5Mo Strength, ksi [MPa] Product Form 5 125] 5 125] 8 200] 5 125] 8 200] 125] 8 200] ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤5 ≤ ≤ ≤ 100][485/345] 70/50 Plate & Bar Mn-0.4Cr-0.4Cu-Si-V 100][485/345] 70/50 Plate & Bar Mn-0.6Cr-0.3Cu-Si-V 100][485/345] 70/50 Plate & Bar Mn-0.5Cr-0.3Cu-Si-V ≤ ≤ ≤ 4 [ 4 [ 4 [ in [mm] in ≤ ≤ ≤ Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) [>100 and [>100 and [>100 and [>100 and [>125 and [>125 and [>100 and [>100 and [>125 and [>125 and [>100 and [>100 and [>125 and [>125 and SteelAlloys and Steel UNS Table C Number 1 K12143 55/33 [380/230] Plate 0.5Cr-0.5Mo or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 33 1 1 1.4 1.4 ASTM ASTM A588 A588 C K K11538 — >4 and 70/50 [485/345] Shapes Mn-0.4Cr-0.4Cu-Si-V 33 1 1 1.4 1.4 ASTM ASTM A588 A588 C C K11538 K11538 >4 and 33 1 1 1.4 1.4 ASTM ASTM A588 A588 B C K12043 K11538 >5 and 3 1 1.4 ASTM A588 B K12043 >4 and 333 1 1 1.4 1 1.4 ASTM 1.4 ASTM ASTM A588 A588 A588 A B B K11430 K12043 K12043 >5 and 70/50 [485/345] Shapes Mn-0.6Cr-0.3Cu-Si-V 3 1 — ASTM/ASME A/SA-335 P15 K11578 60/30 [ 3 1 1.4 ASTM A588 A K11430 >4 and 333 13 13 4.2 1 ASTM/ASME3 1.1 1 A/SA-335 ASTM/ASME3 1.1 1 A/SA-3523 1.1 1 ASTM/ASME ASTM P23 4.2 1 A/SA-369 LC1 ASTM/ASME3 4.2 1 A/SA-369 ASTM/ASME3 1.1 1 K11547 A356 A/SA-387 FP1 J12522 ASTM/ASME 1.1 1 A/SA-426 FP2 ASTM/ASME 4.2 1 2, Cl. A/SA-426 K11522 ASTM/ASME 1.4 A/SA-426 2 CP1 K11547 1.4 CP15 ASTM CP2 J12521 ASTM J12523 J11522 55/30 A588 J11547 A588 55/ 55/30 A A 65/35 [ K11430 65/35 [450/240] 60/30 [ K11430 60/30 [415/ >5 and Castings 70/50 [485/345] C-0.5Mo Shapes Mn-0.5Cr-0.3Cu-Si-V Material Number
121 AWS B2.1/B2.1M-BMG:2014 Nominal Composition 415] Plate C-Mn-Ni-Cr-Cu-V [450/340] Plate C-Mn-Cr-Ni-Cu 33 [380/230] Pipe Fusion Welded 0.5Cr-0.5Mo 45 [485/310] Pipe Fusion Welded 0.5Cr-0.5Mo Minimum Minimum Tensile/Yield 63/42 [435/290]63/42 Plate & Bar Mn-0.6Cr-0.4Cu-Si-Nb Strength, ksi [MPa] Product Form 8 200] ≤ ≤ 100][485/345] 70/50 Plate & Bar Mn-0.6Cr-0.4Cu-Si-Nb ≤ 4 [ in [mm] in ≤ Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) [>125 and [>125 and SteelAlloys and Steel 1202012320 70/40 [485/275] 75/43 [515/295] Plate Plate C-0.5Mo C-0.5Mo UNS 1300513005 85/53 [585/365] 90/65 [620/450] Castings Castings Mn-0.25Mo-V Mn-0.25Mo-V Table C Number 2 K12143 70/45 [485/310] Plate 0.5Cr-0.5Mo or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 333 13 13 1.4 13 1.4 1 11.1 ASTM3 1 ASTM3 1.1 1 ASTM ASTM/ASME3 4.2 1 A588 A/SA-672 ASTM/ASME3 1.1 1 A588 A/SA-691 ASTM/ASME A5953 — 1 A/SA-691 Cl. 1 0.5Cr, L653 — 1 K K121433 1.4 ASTM 2 CM-65 K K118203 1.4 ASTM 2 C AS/NZS K118203 1.1 2 A707 — AS/NZS ASTM/ASME3 4.2 2 A707 A/SA-182 K11526 — ASTM/ASME 36783 1.1 2 A/SA-182 L6, Cl. 1 ASTM/ASME 36783 1.2 2 A/SA-204 L6, Cl. 2 ASTM/ASME F13 1.1 K02902 2 55/ WR350 A/SA-204 ASTM/ASME F23 WR350L0 4.2 K02902 2 65/37 [450/255] A/SA-336 ASTM/ASME3 1.1 B 2 K12822 A/SA-387 65/37 [450/255] — ASTM/ASME —3 1.2 C 2 K12122 A/SA-672 ASTM/ASME Pipe Fusion Welded F13 1.2 2 70/60 [485/415] 2, Cl. K A/SA-672 ASTM/ASME3 4.2 Pipe 70/50 [485/345] Fusion Welded 2 K A/SA-672 H75 ASTM/ASME3 1.2 2 K12520 A/SA-691 60/42 [415/290] L70 ASTM/ASME3 1.2 2 A/SA-691 Tube C-0.5Mo Welded Cl. 2 0.5Cr, 66/52 [455/360] L75 K12021 ASTM/ASME3 — 3 A/SA-691 C-0.5Mo K12143 K12020 70/40 [485/275] 4.2 3 Shapes CM-70 K12320 70/40 [485/275] 4.1 65/50 [450/340] ASTM 3 65/50 CM-75 Forgings ASTM K12020 2.1 Forgings ASTM/ASME ASTM K12320 2.1 A707 C Low A/SA-487 Mn-0.6Cr-0.4Cu-Si-Nb 70/40 [485/275] ASTM/ASME Forgings A871 A/SA-487 ForgingsA 2, Cl. A108 75/45 [515/310] Plate L6, Cl. 3 2Mn-0.3Mo-Cb B 2, Cl. 70/ 70/40 [485/275] J 2Mn-0.3Mo-Cb K02902 60 CW 8620 75/43 [515/295] Pipe Fusion Welded Forgings J 70/40 [485/275] G86200 Pipe Fusion Welded C-0.5Mo 75/43 [515/295] 0.5Cr-0.5Mo Pipe Fusion Welded C-Mn-Cr-Ni-Cu — Pipe Fusion Welded Mn-0.5Mo Pipe Fusion Welded C-0.5Mo C-0.5Mo C-0.5Mo 75/60 [515/415] C-0.5Mo C-0.5Mo [–/–] –/– Forgings 75/60 [515/ 2Mn-0.3Mo-Cb Bar 0.5Ni-0.5Cr-Mo 3 1 1.4 ASTM A588 K — >5 and Material Number
122 AWS B2.1/B2.1M-BMG:2014 Nominal Composition eeeee Mn-0.5Mo-0.5Ni e Mn-0.5Mo-0.5Ni e Mn-0.5Mo-0.75Ni e Mn-0.5Mo-0.75Ni Mn-0.5Mo-0.25Ni Mn-0.5Mo-0.25Ni Mn-0.5Mo-0.75Ni Mn-0.5Mo-0.75Ni Fusion Welded PipeFusion Welded PipeFusion Welded Mn-0.5Mo-0.75Ni Mn-0.5Mo-0.75Ni 450] Plate C-Mn-Ni-Cr-Cu-V 60 [620/415]60 [620/415]50 [550/345]65 [620/450]50 [550/345] Castings65 [620/450] Castings70 [620/485] Forgings Forgings 0.5Ni-0.5Cr-0.25Mo-V Forgings 0.5Ni-0.5Cr-0.25Mo-V Forgings 0.75Ni-0.5Mo-0.3Cr-V Forgings 0.75Ni-0.5Mo-0.3Cr-V 0.75Ni-0.5Mo-Cr-V 0.75Ni-0.5Mo-Cr-V 3.5Ni-1.75Cr-0.5Mo-V 50 [550/345]65 [620/450] Forgings70 [620/485] Forgings 0.75Ni-0.5Mo-0.3Cr-V 0.75Ni-0.5Mo-0.3Cr-V Plate 2.75Ni-1.5Cr-0.5Mo Minimum Minimum Tensile/Yield 80/50 [550/345]90/65 [620/450]90/70 [620/485] Forgings Forgings Plate 0.5Ni-0.5Mo-V 0.5Ni-0.5Mo-V 3Ni-1.75Cr-0.5Mo Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 12539 80/50 [550/345] Plat 12539125541255412529125291255412554 90/70 [620/485] 80/50 [550/345] 90/70 [620/485] 80/50 [550/345] 90/70 [620/485] Plat 80/50 [550/345] Plat 90/70 [620/485] Plat Plat Plat Plat Plat 11597 60/30 [415/205] Forgings 1.25Cr-0.5Mo-Si UNS Table C Number 12 K12521 K12521 80/50 [550/345] 90/70 [620/485] Plate Plate Mn-0.5Mo Mn-0.5Mo or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 333 33 33 3.1 3 ASTM/ASME3 3.1 3 A/SA-487 ASTM/ASME3 3.1 3 A/SA-508 ASTM/ASME3 3.1 3C 4, Cl. A/SA-508 ASTM/ASME3 3.1 3 2, Cl. 1 A/SA-508 ASTM/ASME J13047 3.1 3 2, Cl. 2 A/SA-508 ASTM/ASME K12766 3.1 3 3, Cl. 1 A/SA-508 ASTM/ASME K12766 3.1 3, Cl. 2 A/SA-533 ASTM/ASME K12042 3.1 4N, Cl. 3 A/SA-533 ASTM/ASME K12042 A, Cl. K22375 A/SA-533 A, Cl. 1 B, Cl. 90/ 80/ K 90/ 80/ 90/ 90/ 3 3 3.1 ASTM/ASME A/SA-487A 4, Cl. J13047 90/ 333 33 33 3.1 3 ASTM/ASME3 3.1 3 A/SA-533 ASTM/ASME3 3.1 3 A/SA-533 ASTM/ASME3 3.1 32 B, Cl. A/SA-533 ASTM/ASME3 3.1 31 C, Cl. A/SA-533 K ASTM/ASME3 3.1 32 C, Cl. A/SA-533 K ASTM/ASME3 3.1 31 D, Cl. A/SA-533 K ASTM/ASME3 4.2 32 D, Cl. A/SA-533 K ASTM/ASME3 4.2 3 E, Cl. 1 A/SA-541 K ASTM/ASME3 4.1 3 E, Cl. 2 A/SA-541 K ASTM/ASME3 4.1 3 2, Cl. 1 A/SA-541 K ASTM/ASME 3.1 3 2, Cl. 2 A/SA-541 ASTM/ASME K12765 3.1 3 3, Cl. 1 A/SA-543 ASTM/ASME K12765 1.2 3, Cl. 2 A/SA-543 ASTM/ASME K12045 3.13 B, Cl. A/SA-672 ASTM/ASME K12045 3 C, Cl. A/SA-672 K42339 H80 — J80 80/ K12022 90/ — 90/ 80/50 [550/345] Pipe Fusion Welded 80/50 [550/345] Mn-0.5Mo 333 34 3 3.1 4 ASTM/ASME 4.2 1 A/SA-672 — ASTM 5.1 J90 ASTM/ASME ASTM A/SA-182 A871 F11, Cl.1 A707 — K 65 L6, Cl. 4 K02902 — 90/70 [620/485] 90/75 [620/515] 80/65 [550/ Forgings 2Mn-0.3Mo-Cb Material Number
123 AWS B2.1/B2.1M-BMG:2014 Nominal Composition pe 1.25Cr-0.5Mo-Si Pipe 1Cr-0.5Mo 415/205] Seamless Tube 1.25Cr-0.5Mo-Si 415/205] Seamless Pi [415/220][485/275][485/275] Seamless Tube Castings Castings 1Cr-0.5Mo [415/205] 1Ni-0.5Cr-0.5Mo 0.75Ni-1Mo-0.75Cr Tube E.R.W. 1.25Cr-0.5Mo-Si [415/220] Seamless 45 [515/310]47 [585/325] Plate Plate40 [485/275]30 [415/205]40 [485/275]45 [515/310] 0.5Cr-1.25Mn-Si Castings Piping Fittings 0.5Cr-1.25Mn-Si Piping Fittings Piping Fittings 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo 1.25Cr-0.5Mo-Si Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 1157211572 70/40 [485/275] 75/45 [515/310] Forgings Forgings 1.25Cr-0.5Mo-Si 12062 1.25Cr-0.5Mo-Si 12062 60/32 [415/220] 70/40 [485/275] Piping Fittings Piping Fittings 1Cr-0.5Mo 1Cr-0.5Mo 115971157211572 60/30 [415/205] 70/40 [485/275] 75/45 [515/310] Forgings Forgings Forgings 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si UNS Table C Number 12 K11562 K11564 60/32 [415/220] 70/40 [485/275] Forgings Forgings 1Cr-0.5Mo 1Cr-0.5Mo or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 444 14 14 5.1 1 ASTM/ASME4 5.1 1 A/SA-182 ASTM/ASME4 5.1 1 A/SA-182 ASTM/ASME Cl. F11, 34 5.1 1 A/SA-182 Cl. F12, 4 4.2 1 K ASTM/ASME ASTM Cl. F12, 4 4.2 1 A/SA-202 ASTM/ASME4 5.1 1 A/SA-202 ASTM/ASME4 5.1 1 A199 A/SA-213 ASTM/ASME4 9.1 A 1 A/SA-213 ASTM/ASME4 4.2 B 1 A/SA-217 T11 ASTM/ASME4 5.1 1 T11 K11742 A/SA-217 T12 ASTM/ASME4 5.1 1 K12542 A/SA-217 WC4 K11597 ASTM/ASME4 5.1 1 K11597 A/SA-234 WC5 K11562 ASTM/ASME4 5.1 1 A/SA-234 WC6 J12082 WP11, Cl. 1 ASTM/ASME4 5.1 1 A/SA-234 J22000 WP11, Cl. 2 ASTM/ASME 5.1 1 — A/SA-234 J12072 WP11, Cl. 3 ASTM/ASME 5.1 1 — A/SA-234 WP12, Cl. 1 ASTM/ASME 5.1 75/ — A/SA-250 K WP12, Cl. 2 ASTM/ASME 5.1 85/ 60/30 [ A/SA-250 K ASTM/ASME 60/25 [415/170] 60/32 A/SA-335 T11 70/40 T12 70/40 P11 K11597 Seamless Tube 70/ 60/ K11562 70/ K11597 75/ 1.25Cr-0.5Mo-Si 60/30 60/32 [415/220] 60/30 [ Tube E.R.W. 1Cr-0.5Mo 4 1 5.1 ASTM/ASME A/SA-182 Cl. F11, 2 K 444 14 14 5.1 1 ASTM/ASME4 5.1 1 A/SA-335 ASTM/ASME4 5.1 1 A/SA-336 ASTM/ASME4 5.1 1 A/SA-336 P12 ASTM/ASME Cl. F11, 14 5.1 1 A/SA-336 ASTM/ASME Cl. F11, 2 5.1 1 K A/SA-336 K11562 Cl. F11, 3 6.2 1 K ASTM 6.2 K F12 ASTM 5.1 ASTM/ASME ASTM A356 A/SA-369 K11564 A356 A356 FP11 60/32 6 K11597 8 9 J12073 J11697 70/40 [485/275] J21610 60/30 [415/205] Forgings 70/45 [485/310] 80/50 [550/345] Pipe Forged 85/60 [585/415] 1Cr-0.5Mo Castings Castings 1.25Cr-0.5Mo-Si Castings 1.25Cr-0.5Mo 1Cr-1Mo-V 1Cr-1Mo-V Material Number
124 AWS B2.1/B2.1M-BMG:2014 Nominal Composition 46Fe-24Ni-21Cr-6Mo-Cu-N p 27Ni-22Cr-7Mo-Mn-Cu ate, Sheet, & Strip 27Ni-22Cr-7Mo-Mn-Cu amless & Welded Pipe amless & Welded 0.75Cr-0.75Ni-Cu-Al Plate, Sheet, & Stri amless & Welded Tubeamless & Welded Tubeamless & Welded 0.75Cr-0.5Ni-Cu 0.75Ni-0.5Cu-Mo 345]275] Seamless PipePipe Cast Centrifugal 1.25Cr-0.5Mo 1.25Cr-Mo 415/205]Pipe Cast Centrifugal 1Cr-0.5Mo [450/195] Castings 35Ni-15Cr-0.5Mo 35 [415/240]45 [515/310]33 [380/230] Pipe Fusion Welded 40 [450/275] Pipe Fusion Welded Pipe Fusion Welded 1.25Cr-0.5Mo-Si Pipe Fusion Welded 1.25Cr-0.5Mo-Si 1Cr-0.5Mo 1Cr-0.5Mo Minimum Minimum Tensile/Yield 80/50 [550/345] Forgings70/45 [485/310] 1.25Cr-0.5Mo-Si Bar 1.25Cr-0.5Mo Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 1178911789 60/35 [415/240] 75/45 [515/310] Plate Plate 1.25Cr-0.5Mo-Si 1.25Cr-0.5Mo-Si UNS Table C Number 12 K11757 K11757 55/33 [380/230] 65/40 [450/275] Plate Plate 1Cr-0.5Mo 1Cr-0.5Mo 3MN J94651 80/38 [550/260] Castings or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 44 1 1 5.1 ASTM/ASME 5.1 A/SA-387 ASTM/ASME A/SA-3872 11, Cl. 12, Cl. K 44 2 3 5.1 ASTM/ASME — A/SA-423 ASTM 2 A148 K11540 90-60 D50600 60/37 [415/255] Se 90/60 [620/415] Castings C 44 1 14 5.1 ASTM/ASME4 5.1 A/SA-369 ASTM/ASME4 1 A/SA-3874 1 FP12 5.11 11, Cl. 1 ASTM/ASME 6.2 1 K11562 A/SA-387 K 6.2 ASTM 6.2 12, Cl. ASTM ASTM A389 A389 A405 60/32 [415/220] C23 C24 P24 J12080 J12092 Pipe Forged K11591 1Cr-0.5Mo 70/40 [485/275] 80/50 [550/345] 80/50 [550/ Castings Castings 1.25Cr-0.5Mo-V 1Cr-1Mo-V 444 14 14 5.1 1 ASTM/ASME4 5.1 1 A/SA-426 ASTM/ASME4 5.2 1 A/SA-426 ASTM/ASME4 5.1 1 A/SA-541 CP11 ASTM/ASME4 5.1 1 A/SA-691 CP12 ASTM/ASME4 5.14 11, Cl. 11 1.25CR, Cl. A/SA-691 J12072 ASTM/ASME 5.1 K11789 22 1.25CR, Cl. J11562 A/SA-691 K11572 ASTM/ASME 5.1 K11789 2 A/SA-691 1CR, Cl. 1 ASTM/ASME 4.1 A/SA-739 1CR, Cl. 2 ASTM/ASME 5.1 K11757 A/SA-333 ASTM/ASME K11757 A/SA-423 B11 4 70/40 [485/ 60/ K11797 1 60/30 [ 75/ K11267 K11535 55/ 65/ 60/35 [415/240] 60/37 [415/255] Se Se 45 45 ASTM/ASME A/SA-351 HT30 N08603 65/28 4545 8.2 ASTM/ASME 8.2 A/SA-240 ASTM/ASME A/SA-351 S31277 CN S31277 112/52 [770/360] 45 8.2 ASTM/ASME A/SA-240 — S31277 112/52 [770/360] Pl 5A5A 15A 15A 5.2 15A ASTM/ASME 5.2 1 A/SA-182 ASTM/ASME 5.2 1 A/SA-182 ASTM/ASME — A/SA-182 F21 Cl. F22, 1 5.2 Cl. F22, 3 ASTM K21590 K31545 ASTM K21590 A199 A199 T21 T22 60/30 [415/205] K31545 75/45 [515/310] 75/45 [515/310] K21590 Forgings Forgings Forgings 60/25 [415/170] 60/25 [415/170] 2.25Cr-1Mo 2.25Cr-1Mo 3Cr-1Mo Seamless Tube Seamless Tube 3Cr-1Mo 2.25Cr-1Mo Material Number
125 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Pipe 3Cr-1Mo Pipe 2.25Cr-1Mo amless Tube 2.25Cr-0.5Mo-0.75Si 415/205]485/275]Pipe Cast Centrifugal Pipe Cast Centrifugal 3Cr-1Mo 2.25Cr-1Mo 30 [415/205]30 [415/205] Seamless Tube Seamless Tube30 [415/205] 3Cr-1Mo 2.25Cr-1Mo Seamless 30 [415/205] Seamless Minimum Minimum Tensile/Yield 60/30 [415/205]75/45 [515/310] Pipe Fusion Welded Pipe Fusion Welded 2.25Cr-1Mo 2.25Cr-1Mo Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 2159021590 60/30 [415/205] 75/45 [515/310] Piping Fittings Piping Fittings 2.25Cr-1Mo 2.25Cr-1Mo UNS Table C Number 12 K21590 K21590 60/30 [415/205] 75/45 [515/310] Plate Plate 2.25Cr-1Mo 2.25Cr-1Mo . 1. 2 K31545 K31545 60/30 [415/205] 75/45 [515/310] Plate Plate 3Cr-1Mo 3Cr-1Mo or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 5A 1 — ASTM A199 T4 K31509 60/25 [415/170] Se 5A5A 15A 15A — 15A 5.2 15A — ASTM 15A ASTM 5.2 15A ASTM/ASME 5.2 ASTM 15A A200 A/SA-213 ASTM/ASME 5.2 15A A200 A/SA-213 ASTM/ASME 5.2 1 A200 A/SA-217 T21 ASTM/ASME 5.2 1 T21 A/SA-234 T22 ASTM/ASME 5.2 T22 A/SA-234 WC9 Cl. 1 WP22, K31545 ASTM/ASME 5.2 K31545 A/SA-250 T4 K Cl. 3 WP22, K21590 ASTM/ASME K21590 A/SA-335 K J21890 T22 K31509 P21 K21590 K31545 60/ 60/25 [415/170] 60/ 60/25 [415/170] 70/40 [485/275] 60/25 [415/170] 60/30 [415/205] Tube Castings Tube 60/ Tube Tube E.R.W. 2.25Cr-1Mo 3Cr-1Mo 2.25Cr-1Mo 2.25Cr-0.5Mo-0.75Si 2.25Cr-1Mo 5A 1 5.2 ASTM/ASME A/SA-335 P22 K21590 60/ 5A5A 15A 15A 5.2 15A ASTM/ASME 5.2 15A A/SA-336 ASTM/ASME 5.2 15A A/SA-336 ASTM/ASME Cl. F21, 1 5.2 15A A/SA-336 ASTM/ASME Cl. F21, 3 5.2 1 K315455A A/SA-336 Cl. F22, 1 5.2 1 K315455A ASTM/ASME ASTM Cl. F22, 3 5.2 1 K215905A A/SA-369 ASTM/ASME 5.2 1 K215905A A/SA-369 ASTM/ASME 5.2 15A A356 A/SA-387 FP21 ASTM/ASME 5.2 15A A/SA-387 FP22 ASTM/ASME 5.2 21, Cl 15A K31545 A/SA-387 60/30 [415/205] ASTM/ASME 5.2 21, Cl 15A 10 K21590 A/SA-387 75/45 [515/310] ASTM/ASME 5.2 22, Cl. 15A A/SA-426 60/30 [415/205] ASTM/ASME 5.2 22, Cl. 1 A/SA-426 J22090 75/45 [515/310] ASTM/ASME 5.2 1 A/SA-691 CP21 Forgings ASTM/ASME 5.21 2.25CR, Cl. A/SA-691 CP22 Forgings ASTM/ASME 5.2 K21590 2 2.25CR, Cl. A/SA-691 J31545 Forgings ASTM/ASME 60/30 [415/205] K21590 J21890 A/SA-691 3CR, Cl. 1 Forgings 60/30 [415/205] 3CR, Cl. 2 K31545 K31545 3Cr-1Mo 85/55 [585/380] Pipe Forged 3Cr-1Mo 2.25Cr-1Mo Pipe Forged 2.25Cr-1Mo 60/30 [ 70/40 [ Castings 3Cr-1Mo 60/30 [415/205] 2.25Cr-1Mo 75/45 [515/310] Pipe Fusion Welded Pipe Fusion Welded 2.25Cr-1Mo 3Cr-1Mo 3Cr-1Mo Material Number
126 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Pipe 5Cr-0.5Mo Pipe 5Cr-0.5Mo-Si Pipe 5Cr-0.5Mo-Ti Pipe 9Cr-1Mo 170] Seamless Tube 5Cr-0.5Mo [415/205][415/205][415/205] Seamless Tube Seamless Tube Seamless Tube 5Cr-0.5Mo 5Cr-0.5Mo-Si 5Cr-0.5Mo-Ti [415/205] Seamless [415/205] Seamless [415/205] Seamless 30 [415/205] Seamless Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 41545415459094190941 60/30 [415/205] 75/45 [515/310] 60/30 [415/205] 75/45 [515/310] Piping Fittings Piping Fittings Piping Fittings Piping Fittings 5Cr-0.5Mo 5Cr-0.5Mo 9Cr-1Mo 9Cr-1Mo UNS Table C Number 12 K41545 K41545 60/30 [415/205] 75/45 [515/310] Plate Plate 5Cr-0.5Mo 5Cr-0.5Mo . 1. 2 K90941 K90941[415/205] 60/30 [515/310] 75/45 Plate Plate 9Cr-1Mo 9Cr-1Mo or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 5B5B 15B 15B 5.3 15B ASTM/ASME 5.3 15B A/SA-182 ASTM/ASME 5.4 15B A/SA-182 ASTM/ASME 5.3 15B A/SA-182 F5 5.4 15B F5a ASTM 5.3 15B ASTM/ASME ASTM F9 5.3 15B K41545 A/SA-213 ASTM/ASME K42544 5.3 15B A199 A/SA-213 ASTM/ASME 5.4 15B K90941 A199 A/SA-213 ASTM/ASME T5 5.4 15B A/SA-213 T5b ASTM/ASME 5.3 15B T5 A/SA-217 T5c ASTM/ASME 5.3 1 K415455B T9 A/SA-217 K51545 ASTM/ASME T9 5.3 1 A/SA-234 K41545 C12 70/40 [485/275] ASTM/ASME K41245 5.4 1 A/SA-234 90/65 [620/450] K815901 Cl. WP5, ASTM/ASME C5 5.4 K90941 A/SA-2343 Cl. WP5, 85/55 [585/380] K ASTM/ASME J82090 5.3 A/SA-2341 Cl. WP9, K ASTM/ASME J42045 A/SA-3353 Cl. WP9, K Forgings Forgings 60/30 K 60/30 Forgings P5 60/25 [415/ 60/30 60/25 [415/170] 60/30 [415/205] K41545 90/60 [620/415] 5Cr-0.5Mo 5Cr-0.5Mo 90/60 [620/415] Seamless Tube Seamless Tube 9Cr-1Mo Castings Castings 9Cr-1Mo 60/30 9Cr-1Mo 9Cr-1Mo 5Cr-0.5Mo 5B 1 5.3 ASTM/ASME A/SA-335 P5b K51545 60/30 5B 1 5.3 ASTM/ASME A/SA-335 P5c K41245 60/30 5B5B 15B 1 5.3 1 ASTM/ASME 5.4 A/SA-387 ASTM/ASME 5.4 A/SA-387 ASTM/ASME 5, Cl. A/SA-387 9, Cl 9, Cl 5B5B 15B 15B 5.4 15B ASTM/ASME 5.3 15B A/SA-335 ASTM/ASME 5.3 15B A/SA-336 ASTM/ASME 5.4 1 A/SA-336 ASTM/ASME P9 5.3 1 A/SA-336 ASTM/ASME F5 5.4 A/SA-369 F5A ASTM/ASME 5.3 K90941 A/SA-369 ASTM/ASME F9 K41545 A/SA-387 K42544 FP5 FP9 K90941 5, Cl. K41545 K90941 60/ 60/36 [415/250] 80/50 [550/345] 85/55 [585/380] 60/30 [415/205] 60/30 [415/205] Forgings Forgings Forgings Pipe Forged Pipe Forged 5Cr-0.5Mo 5Cr-0.5Mo 5Cr-0.5Mo 9Cr-1Mo 9Cr-1Mo 5A 1 5.2 ASTM/ASME A/SA-739 B22 K21390 75/45 [515/310] Bar 2.25Cr-1Mo Material Number
127 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Centrifugal Cast Pipe Cast Centrifugal 5Cr-1.5Si-0.5Mo 620/415]620/415]Pipe Cast Centrifugal Pipe Cast Centrifugal 5Cr-0.5Mo 9Cr-1Mo Minimum Minimum Tensile/Yield 85/60 [585/415]85/60 [585/415]85/60 [585/415] Plate Plate Plate 3Cr-1Mo-0.25V-Cb-Ca 3Cr-1Mo-V-Ti-B 2.25Cr-1Mo-V Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 3183031830 85/55 [585/380] 85/60 [585/415] Plate Plate 3Cr-1Mo-V-Ti-B 3Cr-1Mo-V-Ti-B UNS Table C K21590K21590K31835 85/60 [585/415] 85/60 [585/415] Plate 85/60 [585/415] Plate Plate 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo-V Number 3 K215903 K21390 85/55 [585/380] 85/55 [585/380] Forgings Forgings 2.25Cr-1Mo 2.25Cr-1Mo 4 K21590 85/55 [585/380] Plate 2.25Cr-1Mo 4 K21590 85/55 [585/380] Plate 2.25Cr-1Mo or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 5C 1 5.25C ASTM/ASME5C A/SA-542 14a A, Cl. 1 6.2 ASTM/ASME 6.3 A/SA-542 ASTM/ASME A/SA-542 C, Cl. 4a4a D, Cl. K 5C5C 15C 15C 6.2 15C ASTM/ASME 6.2 15C A/SA-508 ASTM/ASME 5.2 15C A/SA-508 ASTM/ASME 5.2 1 A/SA-541 ASTM/ASME 3V 6.2 15C 3VCb A/SA-541 ASTM/ASME 6.2 22, Cl. A/SA-541 ASTM/ASME 5.2 K31830 15C K31390 A/SA-541 22V ASTM/ASME A/SA-542 3V 5.2 1 3VCb K31835 ASTM/ASME5C Cl. A, A/SA-542 6.2 K31830 K31390 ASTM/ASME 1 B, Cl. A/SA-542 85/60 [585/415] 85/60 [585/415] 6.24 C, Cl. ASTM/ASME A/SA-542 K 85/60 [585/415] Cl. E, 4a 85/60 [585/415] Forgings 85/60 [585/415] Forgings K31390 Forgings 3Cr-1Mo-0.25V-Cb-Ca Forgings 3Cr-1Mo-V-Ti-B Forgings 2.25Cr-1Mo-V 3Cr-1Mo-0.25V-Cb-Ca 3Cr-1Mo-V-Ti-B 5B5B 15B 15B 5.3 15C ASTM/ASME 5.4 15C A/SA-426 ASTM/ASME 5.3 15C A/SA-426 ASTM/ASME 5.3 15C A/SA-691 CP5b ASTM/ASME 6.2 15C A/SA-691 CP9 5CR, Cl. 1 ASTM/ASME 6.2 15C J51545 A/SA-182 5CR, Cl. 2 ASTM/ASME 6.2 K41545 15C A/SA-182 ASTM/ASME J82090 6.2 K41545 15C A/SA-182 F22V ASTM/ASME 6.2 1 A/SA-336 F3V ASTM/ASME 6.2 1 F3VCb K31835 A/SA-336 ASTM/ASME 5.2 A/SA-336 F22V K31830 ASTM/ASME K31390 5.2 A/SA-487 F3V ASTM/ASME 60/30 [415/205] F3VCb K31835 A/SA-508 60/30 [415/205] 8, ACl. 75/45 [515/310] 90/60 [ K31830 K31390 22, Cl. J22091 Pipe Fusion Welded 85/60 [585/415] Pipe Fusion Welded 5C 85/60 [585/415] 85/60 [585/415] 5Cr-0.5Mo 85/60 [585/415] 1 5Cr-0.5Mo Forgings 85/60 [585/415] 85/60 [585/415] 5.2 Forgings Forgings 85/55 [585/380] ASTM/ASME5C A/SA-542 Forgings5C B, Cl. 4a 1 Forgings 2.25Cr-1Mo-V Forgings 3Cr-1Mo-0.25V-Cb-Ca 1 3Cr-1Mo-V-Ti-B Castings 6.2 ASTM/ASME 6.2 2.25Cr-1Mo-V A/SA-832 3Cr-1Mo-0.25V-Cb-Ca ASTM/ASME 3Cr-1Mo-V-Ti-B A/SA-832 21V 2.25Cr-1Mo 22V K31830 K31835 5B 1 5.3 ASTM/ASME A/SA-426 CP5 J42045 90/60 [ Material Number
128 AWS B2.1/B2.1M-BMG:2014 Nominal Composition t, & Strip 13Cr t, & Strip 15Cr [450/205][415/205] Plate, Shee Tube Seamless & Welded 13Cr [450/205][415/240] Plate, Shee Tube Seamless & Welded 15Cr [585/415] Plate 3Cr-1Mo-0.25V-Cb-Ca Minimum Minimum Tensile/Yield 105/85 [725/585] Plate 3Cr-1Mo-V-Ti-B 115/100 [795/690]115/100 Plate 3Cr-1Mo-V-Ti-B Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel 31830213902159021590 95/75 [655/515]2159021590 105/85 [725/585] 105/85 [725/585] Plate 105/85 [725/585] Forgings [795/690] 115/100 Plate [795/690] 115/100 Plate 3Cr-1Mo-V-Ti-B 2.25Cr-1Mo Plate Plate 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo 2.25Cr-1Mo UNS 2209122091 105/85 [725/585] 100/75 [690/515] Castings Castings 2.25Cr-1Mo 2.25Cr-1Mo Table C Number .1 S41000 70/40 [485/275] Forgings 13Cr 3 K21590 95/75 [655/515] Plate 2.25Cr-1Mo 3 K21590 95/75 [655/515] Plate 2.25Cr-1Mo . 2 S41000[585/380] 85/55 Forgings 13Cr or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 666 16 16 7.2 1 ASTM/ASME6 7.2 1 A/SA-182 ASTM/ASME6 7.2 1 A/SA-240 ASTM/ASME6 7.2 F6a, Cl 1 A/SA-268 ASTM/ASME6 7.1 1 A/SA-276 4106 7.2 1 TP410 ASTM6 7.1 1 TP410 ASTM/ASME ASTM6 7.2 S41000 2 S41000 A/SA-479 ASTM/ASME6 7.2 2 S41000 A473 A/SA-479 ASTM/ASME6 7.2 2 A473 A/SA-479 403 ASTM/ASME6 7.2 2 A/SA-182 410 ASTM/ASME 7.2 2 403 XM-30 A/SA-240 ASTM/ASME 7.2 S40300 3 410 A/SA-268 F429 7.2 S41040 S41000 S40300 65/30 429 60/30 ASTM 7.2 S41000 TP429 S42900 70/40 [485/275] ASTM/ASME ASTM A/SA-182 S42900 S42900 A473 F6a, Cl A473 70/40 [485/275] 420 Bar 70/40 [485/275] 70/40 [485/275] 70/40 [485/275] 429 70/40 [485/275] 60/35 [415/240] S42000 Bars & Shapes S42900 65/30 60/35 Bars & Shapes Bars & Shapes Forgings Forgings Forgings 13Cr 12Cr 13Cr-Cb 13Cr 70/35 [485/240] 65/35 [450/240] 12Cr 13Cr 15Cr Forgings Forgings 13Cr 15Cr 5C 1 6.2 ASTM/ASME A/SA-832 23V — 85/60 5C5C 35C 35C 5.2 35C ASTM/ASME 5.2 45C A/SA-542 ASTM/ASME 6.2 45C A/SA-542 ASTM/ASME 5.2 45C Cl. A, A/SA-542 ASTM/ASME 5.2 45C B, Cl. A/SA-487 ASTM/ASME 5.2 45C3 C, Cl. A/SA-487 ASTM/ASME 5.2 45CB 8, Cl. A/SA-541 K ASTM/ASME 5.2 55CC 8, Cl. A/SA-542 ASTM/ASME J 6.24 22, Cl. 55C A/SA-542 ASTM/ASME J 5.2 51 Cl. A, A/SA-542 K ASTM/ASME 5.2 51 B, Cl. A/SA-541 K ASTM/ASME 5.21 C, Cl. A/SA-542 K ASTM/ASME 6.25 22, Cl. A/SA-542 K31830 ASTM/ASME2 Cl. A, A/SA-542 K213902 B, Cl. K 2 C, Cl. K K31830 [795/690] 115/100 Forgings 2.25Cr-1Mo Material Number
129 AWS B2.1/B2.1M-BMG:2014 Nominal Composition & Strip 13Cr-4.5Ni-Mo Sheet, & Strip 12Cr-1Al Sheet, & Strip 11Cr-Ti 620] Tube Seamless & Welded 13Cr-4.5Ni-Mo 620]Pipe Seamless & Welded 13Cr-4.5Ni-Mo 620] Plate, Sheet, 415/170] Plate, 380/170] Plate, [795/620][795/620] Bars & Shapes Bars & Shapes 12.5Cr-2Ni-Si 13Cr-4.5Ni-Mo 65 [620/450] Cast Pipe Centrifugal 13Cr Minimum Minimum Tensile/Yield 110/90 [760/620] Fittings 13Cr-4.5Ni-Mo Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C J91150 90/65 [620/450] Castings 13Cr Number B J91540 100/75 [690/515] Castings 13Cr-4Ni A J91540 110/80 [760/550] Castings 13Cr-4Ni D J91171 100/75 [690/515] Castings 13Cr . A J91151 90/65 [620/450] Castings 13Cr-Mo 34 S41000 S41000 110/85 [760/585] [895/760] 130/110 Forgings Forgings 13Cr 13Cr . B. C J91171 J91150[620/450] 90/65 [620/415] 90/60 Castings Castings 13Cr 13Cr or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 666 36 36 7.2 3 ASTM/ASME6 7.2 3 A/SA-182 ASTM/ASME6 7.2 3 A/SA-182 ASTM/ASME F6a, Cl. 7.2 3 A/SA-217 ASTM/ASME 7.2 3 A/SA-336 F6b 7.2 CA15 ASTM/ASME ASTM 7.2 A/SA-426 ASTM/ASME S41026 F6 A/SA-487 CPCA15 A351 CA15 Cl S41000 J911506 CA1566 4 J911506 4 110/90 [760/620]6 7.2 4 ASTM/ASME6 7.2 4 A/SA-268 ASTM/ASME6 85/55 [585/380] 7.2 4 90/ A/SA-3526 7.2 4 S41500 Forgings ASTM/ASME ASTM6 7.2 CA6NM 4 A/SA-479 ASTM/ASME S415006 7.2 4 A/SA-479 J91540 ASTM/ASME6 7.2 Forgings [620/–] 90/– 4 A473 A/SA-487 414 ASTM/ASME6 7.2 4 CA6NM, Cl. S41500 A/SA-487 ASTM/ASME7 7.2 13Cr-0.5Mo 4 CA6NM, Cl. A/SA-731 S41500 7.2 S41400 4 414 ASTM 7.2 1 S41500 Castings ASTM 7.2 S41400 115/90 [795/ 13Cr ASTM/ASME S41500 ASTM 7.1 110/80 [760/550] A743 A/SA-815 ASTM/ASME A743 A/SA-240 S41500 A743 CA40 115/90 115/90 CA6NM 405 S41500 Castings 13Cr J91153 J91540 CB6 S40500 65/35 [450/240] 115/90 [795/ J91804 13Cr-4Ni Forgings 100/70 [690/485] 110/80 [760/550] 60/25 [ 115/85 [795/585] 12.5Cr-2Ni-Si Castings Castings Castings 13Cr-4Ni 13Cr 17Cr-5Ni 6 3 7.2 ASTM/ASME A/SA-182 F6a, Cl. 66 36 36 7.2 ASTM/ASME6 7.2 3 A/SA-487 ASTM/ASME6 3 A/SA-487 CA15 Cl 7.2 4 CA15 Cl. 7.2 4 ASTM 7.2 ASTM/ASME ASTM 7.2 A/SA-182 ASTM/ASME A743 A/SA-240 A743 F6NM S41500 CA15 S41500 CA15M S41500 J91150 J91151 115/90 [795/620] 115/90 [795/ 90/65 [620/450] 90/65 [620/450] Forgings Castings Castings 13Cr-4.5Ni-Mo 13Cr-Mo 13Cr 6 3 7.2 ASTM/ASME A/SA-487 CA15M Cl 7 1 7.1 ASTM/ASME A/SA-240 409 S40910 55/25 [ Material Number
130 AWS B2.1/B2.1M-BMG:2014 Nominal Composition lded Tube 18Cr-2Mo t, & Strip 13Cr t, & Strip 17Cr eet, & Strip 18Cr-Ti-Cb Sheet, & Strip 11Cr-Ti Sheet, & Strip 11Cr-Ti Sheet, & Strip 12Cr-1Ni Sheet, & Strip 12Cr-1Ni Sheet, & Strip 18Cr-Ti Sheet, & Strip 18Cr-2Mo ate, Sheet, & Strip 18Cr-8Ni-2Si 380/170] Plate, 380/170] Plate, 415/205] Tube Seamless & Welded 12Cr-1Al 455/275] Plate, 485/350] Plate, 415/205] Plate, 415/205]415/275] Plate, Sh Plate, [380/205] Tube Seamless & Welded [380/170] Tube Seamless & Welded 12Cr-Ti 11Cr-Ti [415/205] Plate, Shee [450/205] Plate, Shee [415/275][415/240] Seamless & We [415/240] Tube Seamless & Welded [415/205] Tube Seamless & Welded Tube Seamless & Welded 17Cr 18Cr-Ti 18Cr-Ti [415/275][415/205]Pipe Seamless & Welded Pipe Seamless & Welded 18Cr-2Mo 18Cr-Ti Minimum Minimum Tensile/Yield 60/45 [415/310] Bars & Shapes 18Cr-2Mo Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 7 1 7.1 ASTM/ASME A/SA-240 409 S40920 55/25 [ 7 1 7.1 ASTM/ASME A/SA-240 409 S40930 55/25 [ 777 17 17 7.1 1 ASTM/ASME7 7.1 1 A/SA-268 ASTM/ASME7 7.1 1 A/SA-268 ASTM/ASME 7.1 1 S40800 A/SA-268 7.1 1 TP405 ASTM/ASME S40800 ASTM 7.1 TP409 A/SA-479 7.2 S40500 ASTM/ASME ASTM S40900 A473 A/SA-1010 405 A743 40 S40500 405 55/30 CC50 S41003 S40500 60/30 [ 55/25 J92615 60/25 [415/170] 66/40 [ 60/30 [415/205] Bars & Shapes [380/–] 55/– Forgings 12Cr-1Al Castings 12Cr-1Al 28Cr-3Ni 7 1 7.2 ASTM/ASME A/SA-240 410S S41008 60/30 7 1 7.2 ASTM/ASME A/SA-1010 50 S41003 70/50 [ 7 2 7.1 ASTM/ASME A/SA-240 439 S43035 60/30 [ 77 2 2 7.1 ASTM/ASME 7.1 A/SA-182 ASTM/ASME A/SA-240 F430 430 S43000 S43000 60/35 [415/240] 65/30 Forgings 17Cr 77 2 2 7.1 ASTM/ASME 7.1 A/SA-240 ASTM/ASME A/SA-240 S43932 S44400 S43932 S44400 60/30 [ 60/40 [ 777 27 27 7.1 2 ASTM/ASME7 7.1 2 A/SA-268 ASTM/ASME7 7.1 2 A/SA-268 18Cr-2Mo ASTM/ASME7 7.1 2 A/SA-268 ASTM/ASME7 7.1 S44400 2 TP430 A/SA-2687 7.1 TP430Ti 2 ASTM/ASME ASTM7 7.1 2 S43000 TP439 A/SA-479 S43036 ASTM/ASME8 7.1 2 A/SA-479 ASTM/ASME 7.1 2 S43035 A473 A/SA-479 430 ASTM/ASME 7.1 1 A/SA-731 439 ASTM/ASME 7.1 S44400 A/SA-731 60/40 18Cr-2Mo ASTM/ASME 8.1 S43000 430 A/SA-803 S44400 S43035 S44400 TP439 60/35 ASTM 60/35 S43000 TP439 S43035 60/30 S43035 A167 70/40 [485/275] 302B 70/40 [485/275] 60/40 S30215 70/35 [485/240] 60/30 Bars & Shapes 60/30 [415/205] Bars & Shapes Forgings Tube Welded 17Cr 18Cr-Ti 75/30 [515/205] Pl 17Cr 18Cr-Ti 8 1 8.1 ASTM/ASME A/SA-182 F304 S30400 75/30 [515/205] Forgings 18Cr-8Ni Material Number
131 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Minimum Minimum Tensile/Yield 75/30 [515/205]75/30 [515/205]70/25 [485/170] Forgings Forgings80/35 [550/240] Forgings 16Cr-12Ni-2Mo 75/30 [515/205] 16Cr-12Ni-2Mo 70/25 [485/170] Forgings 16Cr-12Ni-2Mo Forgings 16Cr-12Ni-2Mo-N Forgings 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo Strength, ksi [MPa] Product Form 127] 70/30 [485/205] Forgings 16Cr-12Ni-2Mo-N [>127][>127] 70/30 [485/205][>127] 70/30 [485/205] 65/25 [450/170] Forgings[>127] Forgings[>127] 70/30 [485/205] Forgings 16Cr-12Ni-2Mo 65/25 [450/170] 16Cr-12Ni-2Mo [>127] Forgings 16Cr-12Ni-2Mo [>127] 70/30 [485/205] Forgings[>127] 70/30 [485/205][>127] 18Cr-13Ni-3Mo 70/30 [485/205] Forgings 70/30 [485/205] 18Cr-13Ni-3Mo Forgings Forgings 18Cr-10Ni-Ti Forgings 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 5 [>127]5 [>127] 70/30 [485/205] 70/30 [485/205]5 [>127] 65/25 [450/170] Forgings Forgings Forgings 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-182 ASTM/ASME8 8.1 1 A/SA-182 ASTM/ASME8 8.1 1 F304H A/SA-182 ASTM/ASME8 8.1 1 F304H A/SA-182 ASTM/ASME8 8.1 S30409 1 F304L A/SA-182 ASTM/ASME8 8.1 S30409 1 F304L A/SA-182 > ASTM/ASME8 8.1 F304LN 1 S30403 A/SA-182 ASTM/ASME8 8.1 F304LN 1 S30403 A/SA-182 S30453 ASTM/ASME8 8.1 1 F304N A/SA-182 S30453 > ASTM/ASME8 8.1 1 A/SA-182 F316 ASTM/ASME8 8.1 S30451 1 >5 [>127] A/SA-182 F316 ASTM/ASME8 8.1 1 F316H A/SA-182 S31600 75/30 [515/205] ASTM/ASME8 8.1 1 F316H A/SA-182 70/30 [485/205] S31600 70/25 [485/170] ASTM/ASME8 8.1 S31609 1 F316L A/SA-182 ASTM/ASME8 8.1 S31609 1 >5 75/30 [515/205] F316L A/SA-182 ASTM/ASME8 8.1 F316LN 1 S31603 A/SA-182 >5 Forgings ASTM/ASME8 8.1 F316LN 1 S31603 A/SA-182 Forgings S31653 80/35 [550/240] ASTM/ASME Forgings8 8.1 1 F316N A/SA-182 S31653 >5 ASTM/ASME8 8.1 1 >5 [> Forgings A/SA-182 F317 ASTM/ASME8 8.1 S31651 1 A/SA-182 F317 ASTM/ASME8 8.1 1 F317L A/SA-182 S31700 Forgings ASTM/ASME8 8.1 18Cr-8Ni 1 F317L 18Cr-8Ni-N A/SA-182 S31700 ASTM/ASME8 8.1 18Cr-8Ni 1 S31703 >5 A/SA-182 F321 ASTM/ASME 8.1 1 S31703 18Cr-8Ni-N A/SA-182 F321 >5 ASTM/ASME 8.1 1 75/30 [515/205] F321H A/SA-182 S32100 ASTM/ASME 8.1 F321H A/SA-182 S32100 18Cr-8Ni-N ASTM/ASME 8.1 S32109 A/SA-182 F347 ASTM/ASME S32109 >5 A/SA-182 F347 F347H Forgings S34700 >5 F347H S34700 S34709 S34709 >5 75/30 [515/205] >5 16Cr-12Ni-2Mo-N 75/30 [515/205] 75/30 [515/205] Forgings Forgings 75/30 [515/205] Forgings 18Cr-10Ni-Ti 18Cr-10Ni-Ti Forgings 18Cr-10Ni-Cb 18Cr-10Ni-Cb 8 1 8.1 ASTM/ASME A/SA-182 F304 S30400 > Material Number
132 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Sheet, & Strip 17Cr-7Ni 205]205] Seamless Tube Seamless Tube 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo 515/205] Plate, [550/220] Seamless Tube 18Cr-20Ni-5.5Si [515/205][550/240] Seamless Tube Seamless Tube 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 30 [515/205]35 [550/240]30 [515/205]30 [515/205] Seamless Tube25 [485/170] Seamless Tube Seamless Tube Seamless Tube 18Cr-8Ni-N Seamless Tube 18Cr-8Ni-N 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 30 [515/205] 16Cr-12Ni-2Mo 30 [515/205]30 [515/205]30 [515/205] Seamless Tube Seamless Tube30 [515/205] Seamless Tube30 [515/205] Seamless Tube 18Cr-10Ni-Ti 30 [515/205] 18Cr-10Ni-Ti 30 [515/205] Seamless Tube 18Cr-10Ni-Cb Seamless Tube 18Cr-10Ni-Cb Seamless Tube Seamless Tube 18Cr-10Ni-Cb-N 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-18Ni-2Si Minimum Minimum Tensile/Yield 75/30 [515/205]75/30 [515/205]70/25 [485/170] Seamless Tube Seamless Tube Seamless Tube 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 80/30 [550/205] Seamless Tube 18Cr-10Ni-Cb Strength, ksi [MPa] Product Form [>127][>127] 70/30 [485/205] 70/30 [485/205] Forgings Forgings 18Cr-10Ni-Cb 18Cr-10Ni-Cb in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 88 1 1 8.1 ASTM/ASME 8.1 A/SA-182 ASTM/ASME A/SA-182 F348 F348 S34800 S34800 >5 75/30 [515/205] Forgings 18Cr-10Ni-Cb 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-182 ASTM/ASME8 8.1 1 A/SA-182 ASTM/ASME8 8.1 1 F348H A/SA-182 ASTM/ASME8 8.1 1 F348H A/SA-213 ASTM/ASME8 8.1 S34809 1 A/SA-213 F46 ASTM/ASME8 8.1 S34809 1 S32615 A/SA-213 >5 ASTM/ASME8 8.1 1 TP304 A/SA-213 ASTM/ASME S32615 S306008 8.1 TP304H 1 A/SA-213 ASTM/ASME8 8.1 1 S30400 TP304L A/SA-213 S30409 ASTM/ASME TP304LN8 8.1 1 A/SA-213 S30403 ASTM/ASME8 8.1 TP304N 1 S30453 A/SA-213 ASTM/ASME8 8.1 1 TP316 A/SA-213 S30451 75/30 [515/205] ASTM/ASME8 8.1 TP316H 1 A/SA-213 ASTM/ASME8 8.1 1 S31600 TP316L A/SA-213 80/32 78/35 [540/240] S31609 TP316LN8 8.1 1 S31603 ASTM8 8.1 TP316N 1 S31653 Forgings ASTM8 8.1 1 S31651 ASTM/ASME ASTM 75/ 8 8.1 1 A213 A/SA-213 Forgings ASTM/ASME8 8.1 1 A213 80/ A/SA-213 ASTM/ASME8 8.1 1 A213 TP321 TP316Ti A/SA-213 75/ ASTM/ASME8 8.1 TP321H 1 18Cr-10Ni-Cb 75/ A/SA-213 TP317 ASTM/ASME8 S31635 8.1 1 S32100 TP347 70/ A/SA-213 TP317L S32109 ASTM/ASME 75/30 8.1 18Cr-15Ni-4Si TP347H 1 A/SA-213 S31700 TP347HFG ASTM/ASME 8.1 1 S31703 S34700 80/35 A/SA-213 S34709 S34710 ASTM/ASME TP347LN 8.1 A/SA-213 ASTM/ASME 8.1 S34751 TP348 A/SA-213 ASTM/ASME TP348H A/SA-240 S34800 XM-15 75/30 [515/205] S34809 75/ 75/ 301 S38100 75/30 [515/ 75/30 [515/ 75/ 75/ Seamless Tube S30100 75/ 16Cr-12Ni-2Mo-Ti 75/ 75/ 75/ 75/30 [ Material Number
133 AWS B2.1/B2.1M-BMG:2014 Nominal Composition p 17.5Cr-17.5Ni-5.3Si Strip 18Cr-20Ni-5.5Si Strip 18Cr-13Ni-3Mo-N Strip 18Cr-13Ni-3Mo Strip 18Cr-13Ni-3Mo Strip 16Cr-12Ni-2Mo-Ti Strip 16Cr-12Ni-2Mo-N Strip 16Cr-12Ni-2Mo-N Strip 16Cr-12Ni-2Mo Strip 16Cr-12Ni-2Mo Strip 16Cr-12Ni-2Mo eet, & Stripeet, & Strip 18Cr-10Ni-Ti eet, & Strip 18Cr-10Ni-Cb 18Cr-10Ni-Cb eet, & Stripeet, & Strip 18Cr-8Ni-N 18Cr-8Ni-N Sheet, & Strip 18Cr-8Ni Sheet, & Strip 18Cr-8Ni Sheet, & Strip 18Cr-8Ni Sheet, & Strip 18Cr-8Ni Sheet, & Strip 18Cr-11Ni Plate, Sheet, & Stri Plate, Sheet, & Strip 16Cr-12Ni-2Mo-Cb 205] Plate, Sheet, & Strip 18Cr-18Ni-2Si 220] Plate, Sheet, & 240] Plate, Sheet, & 205] Plate, Sheet, & Strip 18Cr-10Ni-Ti 205]205] Plate, Sheet, & Strip240] Plate, Sheet, & Strip 18Cr-10Ni-Cb Plate, Sheet, & Strip 18Cr-10Ni-Cb 18Cr-15Ni-4Si 205] Plate, Sheet, & 205] Plate, Sheet, & 205] Plate, Sheet, & 240] Plate, Sheet, & 205] Plate, Sheet, & 170] Plate, Sheet, & 205] Plate, Sheet, & 205] Plate, Sheet, & 515/205] Plate, Sh 515/205]515/205] Plate, Sh Plate, Sh 515/205] Plate, 515/205] Plate, 515/205] Plate, 485/170] Plate, 515/205]550/240]485/170] Plate, Sh Plate, Sh Plate, 50 [620/345]50 Sheet & Strip 18Cr-8Ni-N Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) 2 85/40 [585/275] Plate 18Cr-8Ni-N SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 1 1 8.1 1 ASTM/ASME 8.1 A/SA-240 ASTM/ASME 8.1 A/SA-240 ASTM/ASME XM-15 A/SA-240 XM-21 S38100 XM-21 S3045 S30452 75/30 [515/ 90/ 8 1 8.1 ASTM/ASME A/SA-240 S32615 S32615 80/32 [550/ 8 1 8.1 ASTM/ASME A/SA-240 S31753 S31753 80/35 [550/ 88 1 1 8.1 ASTM/ASME 8.1 A/SA-240 ASTM/ASME A/SA-240 321 321H S32100 S32109 75/30 [515/ 75/30 [ 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-240 ASTM/ASME 8.1 1 A/SA-240 ASTM/ASME 8.1 1 A/SA-240 347 ASTM/ASME 8.1 A/SA-240 347H ASTM/ASME 8.1 A/SA-240 348 ASTM/ASME S34700 S34709 A/SA-240 348H S30600 S34800 S30601 S34809 S30600 S30601 75/30 [515/ 75/30 [ 75/30 [515/ 75/30 [ 78/35 [540/ 78/37 [540/255] 8 1 8.1 ASTM/ASME A/SA-240 317L S31703 75/30 [515/ 8 1 8.1 ASTM/ASME A/SA-240 317 S31700 75/30 [515/ 8 1 8.1 ASTM/ASME A/SA-240 302 S30200 75/30 [ 8 1 8.1 ASTM/ASME A/SA-240 316Ti S31635 75/30 [515/ 8 1 8.1 ASTM/ASME A/SA-240 304 S30400 75/30 [ 8 1 8.1 ASTM/ASME A/SA-240 316N S31651 80/35 [550/ 8 1 8.1 ASTM/ASME A/SA-240 304H S30409 75/30 [ 8 1 8.1 ASTM/ASME A/SA-240 316LN S31653 75/30 [515/ 8 1 8.1 ASTM/ASME A/SA-240 304L S30403 70/25 [ 8 1 8.1 ASTM/ASME A/SA-240 316L S31603 70/25 [485/ 888 1 1 8.1 1 ASTM/ASME8 8.1 A/SA-240 ASTM/ASME 8.1 A/SA-240 ASTM/ASME 1 304LN A/SA-240 304N 8.1 S30453 305 ASTM/ASME S30451 A/SA-240 S30500 316H S31609 75/30 [ 80/35 [ 70/25 [ 75/30 [515/ 8 1 8.1 ASTM/ASME A/SA-240 316Cb S31640 75/30 [515/205] 8 1 8.1 ASTM/ASME A/SA-240 316 S31600 75/30 [515/ Material Number
134 AWS B2.1/B2.1M-BMG:2014 Nominal Composition less & Welded Tubeless & Welded 16Cr-12Ni-2Mo-N amless & Welded Tubeamless & Welded 18Cr-8Ni-N Tubeamless & Welded Tubeamless & Welded 18Cr-13Ni-3Mo Tubeamless & Welded Tubeamless & Welded 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 30 [515/205]30 [515/205]25 [485/170]30 [515/205] Tube Welded 35 [550/240] Tube Welded 30 [515/205] Tube Welded 30 [515/205] Tube Welded 16Cr-12Ni-2Mo Tube Welded 16Cr-12Ni-2Mo Tube Welded 16Cr-12Ni-2Mo Tube Welded 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo Minimum Minimum Tensile/Yield 75/30 [515/205] Tube Welded 18Cr-18Ni-2Si 75/30 [515/205]75/30 [515/205]75/30 [515/205]75/30 [515/205] Tube Welded Tube Welded Tube Welded Tube Welded 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 18 18 8.1 18 8.1 1 ASTM8 8.1 1 ASTM 8.1 1 ASTM 8.1 1 A269 ASTM 8.1 A269 ASTM 8.1 A269 TP316 ASTM A269 TP316L ASTM A269 TP316LN S31600 S31603 A269 S31653 TP317 A269 TP321 S31700 TP347 S32100 TP348 S34700 S34800 [–/–] –/– 75/30 [515/205] [–/–] –/– Seam 75/30 [515/205] Tube Seamless & Welded 75/30 [515/205] Tube Seamless & Welded Se 75/30 [515/205] 16Cr-12Ni-2Mo Se 75/30 [515/205] 16Cr-12Ni-2Mo Se Se 8 1 8.1 ASTM/ASME A/SA-249 TP XM-15 S38100 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-249 ASTM/ASME8 8.1 1 A/SA-249 ASTM/ASME8 8.1 1 TP304 A/SA-249 ASTM/ASME8 8.1 TP304H 1 A/SA-249 ASTM/ASME8 8.1 1 S30400 TP304L A/SA-249 S30409 ASTM/ASME TP304LN8 8.1 1 A/SA-249 S30403 ASTM/ASME8 8.1 TP304N 1 S30453 A/SA-249 ASTM/ASME8 8.1 1 TP316 A/SA-249 S30451 ASTM/ASME8 8.1 TP316H 1 A/SA-249 ASTM/ASME8 8.1 1 S31600 TP316L A/SA-249 S31609 ASTM/ASME TP316LN8 8.1 1 A/SA-249 S31603 75/30 [515/205] ASTM/ASME8 8.1 TP316N 1 S31653 75/30 [515/205] A/SA-249 ASTM/ASME8 8.1 1 TP317 70/25 [485/170] A/SA-249 S31651 ASTM/ASME 75/30 [515/205]8 8.1 1 TP317L A/SA-249 ASTM/ASME8 8.1 1 S31700 Tube Welded 80/35 [550/240] TP321 A/SA-249 Tube S31703 Welded ASTM/ASME8 8.1 TP321H 1 A/SA-249 Tube 75/ Welded ASTM/ASME 8.1 1 S32100 Tube 75/ Welded TP347 A/SA-249 S32109 ASTM/ASME 8.1 TP347H 1 70/ A/SA-249 Tube Welded 75/ 8.1 S34700 TP348 S34709 18Cr-8Ni ASTM 8.1 TP348H 18Cr-8Ni 80/ ASTM S34800 18Cr-8Ni 18Cr-8Ni-N S34809 75/ ASTM A269 75/ 18Cr-8Ni-N A269 75/30 [515/205] A269 75/30 [515/205] TP304 TP304L TP304LN S30400 S30403 Tube Welded S30453 Tube Welded 18Cr-10Ni-Ti 18Cr-10Ni-Ti –/– [–/–] 75/30 [515/205] –/– [–/–] Se Tube Seamless & Welded Tube Seamless & Welded 18Cr-8Ni 18Cr-8Ni Material Number
135 AWS B2.1/B2.1M-BMG:2014 Nominal Composition amless & Welded Pipe amless & Welded 16Cr-12Ni-2Mo-Ti Seamless & Welded TubeSeamless & Welded 18Cr-8Ni 205]205] Seamless Tube Seamless Tube 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 220]Pipe Seamless & Welded 18Cr-20Ni-5.5Si 205]240]Pipe Seamless & Welded Pipe Seamless & Welded 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 540/240]Pipe Seamless & Welded 18Cr-15Ni-4Si 515/205]550/240]Pipe Seamless & Welded 515/205]Pipe Seamless & Welded 515/205]Pipe Seamless & Welded 485/170] 18Cr-8Ni-N Pipe Seamless & Welded 18Cr-8Ni-N 16Cr-12Ni-2Mo Pipe Seamless & Welded 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 515/205]515/205]Pipe Seamless & Welded Pipe Seamless & Welded 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo [515/205][515/205]Pipe Seamless & Welded [515/205]Pipe Seamless & Welded [485/170]Pipe Seamless & Welded 18Cr-18Ni-2Si Pipe Seamless & Welded 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) 03 75/30 [515/205] 70/25 [485/170] Bar Bar 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo SteelAlloys and Steel 3040030403 75/30 [515/205] 70/25 [485/170] Bar Bar 18Cr-8Ni 18Cr-8Ni UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 18 18 8.1 18 8.1 1 ASTM8 8.1 1 ASTM8 8.1 1 ASTM8 8.1 1 A271 ASTM8 8.1 1 A271 ASTM8 8.1 1 A271 TP304 ASTM8 8.1 1 A271 TP304H ASTM8 8.1 1 A271 S30400 TP316 ASTM/ASME ASTM8 8.1 S30409 1 A271 A/SA-276 TP316H ASTM/ASME8 8.1 1 A271 A/SA-276 S31600 TP321 ASTM/ASME8 8.1 S31609 1 A271 TP304 A/SA-276 TP321H ASTM/ASME8 8.1 1 TP304L A/SA-276 S32100 TP347 ASTM/ASME8 8.1 S32109 1 S TP316 A/SA-312 TP347H S ASTM/ASME8 8.1 1 TP316L A/SA-312 S34700 ASTM/ASME8 8.1 S34709 1 S3160 S30600 75/30 [515/205] A/SA-312 S3160 75/30 [515/205] ASTM/ASME8 8.1 1 S32615 A/SA-312 TP XM-15 ASTM/ASME S306008 8.1 1 75/30 [515/ A/SA-312 75/30 [515/ ASTM/ASME S326158 8.1 S38100 1 TP304 Seamless Tube A/SA-312 ASTM/ASME8 Seamless Tube 8.1 TP304H 1 75/30 [515/205] A/SA-312 75/30 [515/205] ASTM/ASME8 8.1 1 S30400 TP304L A/SA-312 S30409 ASTM/ASME TP304LN8 8.1 1 75/30 [515/205] A/SA-312 S30403 75/30 [515/205] ASTM/ASME 8.1 TP304N 1 S30453 Seamless Tube A/SA-312 18Cr-8Ni ASTM/ASME Seamless Tube 8.1 1 18Cr-8Ni TP316 A/SA-312 78/35 [ S30451 ASTM/ASME 8.1 TP316H Seamless Tube A/SA-312 80/32 [550/ 75/30 ASTM/ASME Seamless Tube 8.1 S31600 TP316L A/SA-312 S31609 TP316LN 18Cr-10Ni-Ti 18Cr-10Ni-Ti S31603 75/30 ASTM TP316N S31653 75/30 18Cr-10Ni-Cb 70/25 18Cr-10Ni-Cb S31651 75/30 [ A312 80/35 [ TP316Ti 75/30 [ 75/30 [ S31635 70/25 [ 75/30 [515/ 80/35 [550/ 75/30 [515/205] Se 8 1 8.1 ASTM A270 TP304 S30400 75/30 [515/205] 88 1 1 8.1 ASTM/ASME 8.1 A/SA-312 ASTM/ASME A/SA-312 TP317 TP317L S31700 S31703 75/30 [ 75/30 [ Material Number
136 AWS B2.1/B2.1M-BMG:2014 Nominal Composition ss Pipe 18Cr-10Ni-Ti ss Pipe 18Cr-10Ni-Ti ss Pipess Pipe 18Cr-10Ni-Ti 18Cr-10Ni-Ti 515/205]515/205]Pipe Seamless & Welded 515/205]Pipe Seamless & Welded 515/205]Pipe Seamless & Welded 18Cr-10Ni-Cb 515/205]Pipe Seamless & Welded 18Cr-10Ni-Cb 18Cr-10Ni-Cb-N Pipe Seamless & Welded 18Cr-10Ni-Cb 18Cr-10Ni-Cb 30 [485/205] Castings 19Cr-9Ni-0.5Mo Minimum Minimum Tensile/Yield 70/30 [485/205]70/30 [485/205]65/25 [450/170]80/35 [550/240] Forgings Forgings Forgings Forgings 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 70/30 [485/205]70/30 [485/205] Castings Castings 19Cr-9Ni-2Mo 16Cr-14Ni-2Mo Strength, ksi [MPa] Product Form 10] 70/25 [485/170] Seamle 10] 70/25 [485/170] Seamle 10] 75/30 [515/205] Seamle 10] 75/30 [515/205] Seamle ≤ ≤ in [mm] in Thickness 0.375 [ 0.375 [ or Diameter or Diameter Limitations, ≤ ≤ .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 8 1 8.1 ASTM/ASME A/SA-312 TP321 S32100 8 1 8.1 ASTM/ASME A/SA-312 TP321 S32100 [> >0.375 8 1 8.1 ASTM/ASME A/SA-312 TP321H S32109 [> >0.375 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-312 ASTM/ASME8 8.1 1 A/SA-312 ASTM/ASME8 8.1 TP321H 1 A/SA-312 ASTM/ASME8 8.1 1 TP347 A/SA-312 S32109 ASTM/ASME8 8.1 TP347H 1 A/SA-312 ASTM/ASME TP347LN8 8.1 1 S34700 A/SA-312 S34709 ASTM/ASME8 8.1 1 S34751 TP348 A/SA-336 ASTM/ASME8 8.1 TP348H 1 A/SA-336 ASTM/ASME8 8.1 1 S34800 A/SA-336 F304 S34809 ASTM/ASME8 8.1 1 F304H A/SA-336 ASTM/ASME8 8.1 1 F304L A/SA-336 S30400 ASTM/ASME8 8.1 S30409 F304LN 1 A/SA-336 75/30 [ ASTM/ASME8 8.1 1 S30403 75/30 [ F304N A/SA-336 S30453 ASTM/ASME 75/30 [ 8 8.1 1 A/SA-336 F316 ASTM/ASME8 8.1 S30451 1 F316H A/SA-336 75/30 [ ASTM/ASME8 8.1 1 75/30 [ F316L A/SA-336 S31600 ASTM/ASME8 8.1 S31609 F316LN 1 A/SA-336 ASTM/ASME8 8.1 1 S31603 70/30 [485/205] F316N A/SA-336 S31653 70/30 [485/205] ASTM/ASME8 8.1 1 A/SA-336 F321 65/25 [450/170] ASTM/ASME8 8.1 S31651 1 70/30 [485/205] F321H A/SA-336 ASTM/ASME8 8.1 1 A/SA-336 S32100 F347 80/35 [550/240] ASTM/ASME 8.1 S32109 1 Forgings F347H A/SA-336 Forgings ASTM/ASME 8.1 1 A/SA-336 S34700 F348 ASTM/ASME Forgings 8.1 S34709 F348H Forgings A/SA-351 ASTM/ASME 8.1 70/30 [485/205] A/SA-351 S34800 F46 Forgings ASTM/ASME S34809 A/SA-351 CF10 CF10M 18Cr-8Ni S30600 18Cr-8Ni CF10MC 70/30 [485/205] J92590 70/30 [485/205] J92901 18Cr-8Ni 18Cr-8Ni-N Forgings J92971 70/30 [485/205] 18Cr-8Ni-N 70/30 [485/205] 70/30 [485/205] Forgings 65/25 [450/170] Forgings 16Cr-12Ni-2Mo-N Forgings 78/32 [540/220] Forgings 70/ Forgings Forgings 18Cr-10Ni-Ti 18Cr-10Ni-Ti Forgings 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-15Ni-4Si Material Number
137 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Pipe 16Cr-8Ni-2Mo PipePipe 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo Pipe 18Cr-8Ni-N Pipe 18Cr-8Ni-N ss Pipe 18Cr-8Ni less Pipe 18Cr-8Ni less Pipe 18Cr-8Ni 515/205]485/170] Pipe Fusion Welded 515/205]550/240] Pipe Fusion Welded 16Cr-12Ni-2Mo Pipe Fusion Welded Pipe Fusion Welded 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N [515/205][550/240] Pipe Fusion Welded [515/205] Pipe Fusion Welded Pipe Fusion Welded 18Cr-8Ni-N 18Cr-8Ni-N 16Cr-12Ni-2Mo 30 [515/205] Seamless 30 [515/205] Seamless 35 [550/240] Seamless 30 [515/205] Seamless 30 [515/205] Seamless Minimum Minimum Tensile/Yield 70/30 [485/205]70/30 [485/205]70/30 [485/205] Castings75/35 [515/240] Castings Castings 18Cr-12Ni-2Mo Castings 18Cr-10Ni-Cb 18Cr-12Ni-2Mo 19Cr-10Ni-3Mo 75/30 [515/205] Seamle Strength, ksi [MPa] Product Form 21] 70/30 [485/205] Seam ≥ [<21] 75/30 [515/205] Seam in [mm] in Thickness 0.812 [ or Diameter or Diameter Limitations, ≥ .2 (Continued) (Continued) SteelAlloys and Steel UNS 9250092600 77/35 [530/240] 77/35 [530/240] Castings Castings 18Cr-8Ni 18Cr-8Ni Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 88 1 1 8.1 ASTM/ASME 8.1 A/SA-351 ASTM/ASME A/SA-351 CF3 CF3A J92500 J 70/30 [485/205] Castings 18Cr-8Ni 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-351 ASTM/ASME8 8.1 1 A/SA-351 ASTM/ASME8 8.1 1 CF3M A/SA-351 ASTM/ASME8 8.1 1 A/SA-351 CF8 ASTM/ASME8 8.1 1 J92800 CF8A A/SA-351 ASTM/ASME8 8.1 1 CF8C A/SA-351 ASTM/ASME J926008 8.1 1 J CF8M A/SA-358 ASTM/ASME8 8.1 1 CG8M J92710 A/SA-358 ASTM/ASME8 8.1 1 J92900 A/SA-358 304 ASTM/ASME8 8.1 J93000 1 A/SA-358 304H ASTM/ASME8 8.1 1 A/SA-358 304L ASTM/ASME8 8.1 S30400 1 304LN S30409 A/SA-358 ASTM/ASME8 8.1 1 A/SA-358 304N S30403 70/30 [485/205] ASTM/ASME8 8.1 S30453 1 A/SA-358 316 ASTM/ASME8 8.1 1 S30451 A/SA-358 316H ASTM/ASME8 8.1 1 A/SA-358 316L ASTM/ASME 8.1 S31600 1 316LN S31609 A/SA-358 Castings ASTM/ASME 8.1 1 A/SA-358 S31603 316N 75/30 [515/205] ASTM/ASME 8.1 S31653 75/30 [515/205] A/SA-358 321 ASTM/ASME 8.1 70/25 [485/170] S31651 A/SA-376 75/30 347 ASTM/ASME Pipe Fusion Welded A/SA-376 Pipe Fusion Welded 348 S32100 16-8-2H 80/35 Pipe Fusion Welded 18Cr-8Ni S34700 TP304 75/30 [ S16800 S34800 75/30 18Cr-8Ni S30400 18Cr-8Ni 70/25 [ 75/30 [ 18Cr-8Ni 80/35 [ 75/30 [515/205] 75/30 [515/205] 75/ 75/30 [515/205] Pipe Fusion Welded Pipe Fusion Welded Pipe Fusion Welded 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-10Ni-Cb 8 1 8.1 ASTM/ASME A/SA-376 TP304 S30400 <0.812 8 1 8.1 ASTM/ASME A/SA-376 TP304H S30409 8 1 8.1 ASTM/ASME A/SA-376 TP304LN S30453 75/ 8 1 8.1 ASTM/ASME A/SA-376 TP304N S30451 80/ 8 1 8.1 ASTM/ASME A/SA-376 TP316 S31600 75/ 8 1 8.1 ASTM/ASME A/SA-376 TP316H S31609 75/ Material Number
138 AWS B2.1/B2.1M-BMG:2014 Nominal Composition ttingsttings 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N pepe 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N FittingsFittingsFittings 18Cr-8Ni-N Fittings 18Cr-8Ni-N Fittings 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo FittingsFittingsFittings 18Cr-13Ni-3Mo Fittings 18Cr-13Ni-3Mo Fittings 18Cr-10Ni-Ti Fittings 18Cr-10Ni-Ti Fittings 18Cr-10Ni-Cb Fittings 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb Pipe 18Cr-10Ni-Cb Pipe 18Cr-10Ni-Cb Pipe 18Cr-10Ni-Cb ng Fittingsng Fittingsng Fittings 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni ss Pipe 18Cr-10Ni-Ti ss Pipess Pipe 18Cr-10Ni-Ti 18Cr-10Ni-Ti ss Pipe 18Cr-10Ni-Ti 515/205]550/240] Wrought Piping Fi Wrought Piping Fi [515/205][550/240] Seamless Pi Seamless Pi [550/240][515/205] Wrought Piping [515/205] Wrought Piping [485/170] Wrought Piping Wrought Piping [515/205][515/205] Wrought Piping [515/205] Wrought Piping [515/205] Wrought Piping [515/205] Wrought Piping [515/205] Wrought Piping [515/205] Wrought Piping [515/205] Wrought Piping Wrought Piping [515/205] Wrought Piping 30 [515/205] Seamless 30 [515/205] Seamless 30 [515/205] Seamless 30 [515/205]25 [485/170] Wrought Pipi Wrought Pipi 30 [515/205] Wrought Pipi Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form 10] 70/25 [485/170] Seamle 10] 70/25 [485/170] Seamle 10] 75/30 [515/205] Seamle 10] 75/30 [515/205] Seamle ≤ ≤ in [mm] in Thickness 0.375 [ 0.375 [ or Diameter or Diameter Limitations, ≤ ≤ .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 8 1 8.1 ASTM/ASME A/SA-376 TP316LN S31653 75/30 888 1 1 8.1 1 ASTM/ASME 8.1 A/SA-376 ASTM/ASME 8.1 A/SA-376 ASTM/ASME TP316N A/SA-376 TP321 S31651 TP321 S32100 S32100 [> >0.375 80/35 88 1 1 8.1 ASTM/ASME 8.1 A/SA-376 ASTM/ASME A/SA-376 TP321H TP321H S32109 S32109 [> >0.375 8 1 8.1 ASTM/ASME A/SA-376 TP347 S34700 75/ 8 1 8.1 ASTM/ASME A/SA-376 TP347H S34709 75/ 8 1 8.1 ASTM/ASME A/SA-376 TP348 S34800 75/ 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-403 ASTM/ASME8 8.1 1 A/SA-403 ASTM/ASME8 8.1 WP304N 1 A/SA-403 ASTM/ASME8 8.1 1 WP316 S30451 A/SA-403 ASTM/ASME8 8.1 WP316H 1 A/SA-403 ASTM/ASME S316008 8.1 WP316L 1 S31609 A/SA-403 WP316LN ASTM/ASME8 8.1 1 S31603 A/SA-403 ASTM/ASME8 8.1 S31653 WP316N 1 A/SA-403 ASTM/ASME8 8.1 1 WP317 S31651 A/SA-403 ASTM/ASME8 8.1 WP317L 1 A/SA-403 ASTM/ASME S317008 8.1 80/35 1 WP321 S31703 A/SA-403 ASTM/ASME 8.1 WP321H 1 A/SA-403 75/30 ASTM/ASME S32100 8.1 75/30 1 WP347 S32109 A/SA-403 ASTM/ASME 8.1 WP347H 70/25 A/SA-403 75/30 [ ASTM/ASME S34700 8.1 WP348 S34709 A/SA-409 ASTM/ASME WP348H 80/35 [ A/SA-409 S34800 TP304 S34809 75/30 TP304L 75/30 S30400 75/30 S30403 75/30 75/30 75/30 75/30 75/30 75/30 [515/205] 70/25 [485/170] Pipe Welded Pipe Welded 18Cr-8Ni 18Cr-8Ni 888 1 1 8.1 1 ASTM/ASME 8.1 A/SA-403 ASTM/ASME 8.1 A/SA-403 ASTM/ASME WP304H A/SA-403 WP304L S30409 WP304LN S30403 S30453 75/ 70/ 75/30 8 1 8.1 ASTM/ASME A/SA-403 WP304 S30400 75/ Material Number
139 AWS B2.1/B2.1M-BMG:2014 Nominal Composition ntrifugal Cast Pipe Cast ntrifugal 16Cr-12Ni-2Mo 205]Pipe Cast Centrifugal 205] 16Cr-12Ni-2Mo Pipe Cast Centrifugal 18Cr-12Ni-2Mo 485/205]485/205]530/240]Pipe Cast Centrifugal Pipe Cast Centrifugal 485/205]Pipe Cast Centrifugal 16Cr-14Ni-2Mo 530/240]485/205]Pipe Cast Centrifugal 18Cr-8Ni Pipe Cast Centrifugal 18Cr-8Ni Pipe Cast Centrifugal 18Cr-8Ni 18Cr-8Ni 18Cr-10Ni-Cb 30 [515/205]25 [485/170]30 [515/205] Pipe Welded Pipe Welded Pipe Welded 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 18Cr-13Ni-3Mo Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-409 ASTM/ASME8 8.1 1 A/SA-409 ASTM/ASME8 8.1 1 TP316L A/SA-409 ASTM/ASME8 8.1 1 TP317 A/SA-409 S31603 ASTM/ASME8 8.1 1 TP321 A/SA-4098 8.1 1 S31700 TP347 ASTM8 8.1 1 S32100 TP348 ASTM8 8.1 1 S34700 ASTM8 8.1 1 S34800 A430 ASTM8 8.1 1 A430 ASTM8 8.1 1 FP16-8-2H A430 70/ ASTM8 8.1 1 A430 S16800 FP304 75/ ASTM8 8.1 1 A430 FP304H 75/30 [515/205] ASTM8 8.1 1 A430 FP304N S30400 75/30 [515/205] ASTM8 8.1 S30409 1 A430 FP316 75/30 [515/205] ASTM8 8.1 S30451 1 A430 FP316H ASTM/ASME ASTM8 8.1 1 A430 Pipe Welded A/SA-451 FP316N S31600 ASTM/ASME8 8.1 S31609 1 A430 Pipe Welded A/SA-451 CPF10MC FP321 ASTM/ASME8 8.1 70/30 [485/205] S31651 1 A430 Pipe Welded A/SA-451 FP321H ASTM/ASME8 8.1 J92971 1 CPF3 A/SA-451 S32100 FP347 ASTM/ASME8 8.1 S32109 1 CPF3A 70/30 [485/205] 18Cr-10Ni-Ti A/SA-451 FP347H 70/30 [485/205] ASTM/ASME8 8.1 1 CPF3M 18Cr-10Ni-Cb J92500 A/SA-451 Pipe Forged S34700 75/35 [515/240] ASTM/ASME8 8.1 J92500 S34709 1 18Cr-10Ni-Cb A/SA-451 CPF8 ASTM/ASME J92800 8.1 1 CPF8A 70/30 [485/205] A/SA-451 70/30 [485/205] Pipe Forged 8.1 1 CPF8C Pipe Forged J92600 75/35 [515/240] ASTM 8.1 J92600 CPF8M Pipe Forged 16Cr-8Ni-2Mo 70/30 [ ASTM 8.1 J92710 70/30 [485/205] 70/30 [485/205] Pipe J92900 Forged ASTM A452 Pipe Forged ASTM 70/30 [ A452 70/30 [485/205] Pipe Forged 18Cr-8Ni 77/35 [ 70/30 [485/205] 18Cr-8Ni A452 TP304H 70/30 [485/ 18Cr-8Ni-N Pipe Forged A473 Pipe Forged TP316H 16Cr-12Ni-2Mo S30409 16Cr-12Ni-2Mo 70/30 [ TP347H 77/35 [ 16Cr-12Ni-2Mo-N Pipe Forged S31609 Pipe Forged 70/30 [ S34709 302 70/30 [485/ 18Cr-10Ni-Ti 18Cr-10Ni-Ti S30200 18Cr-10Ni-Cb 18Cr-10Ni-Cb 75/30 [515/205] 75/30 [515/205] 75/30 [515/205] Cast Pipe Centrifugal Ce Cast Pipe Centrifugal 75/30 [515/205] 18Cr-8Ni 18Cr-10Ni-Cb Forgings 18Cr-8Ni 8 1 8.1 ASTM/ASME A/SA-409 TP316 S31600 75/ Material Number
140 AWS B2.1/B2.1M-BMG:2014 Nominal Composition [515/205][485/170][515/205] Bars & Shapes[550/240] Bars & Shapes 16Cr-12Ni-2Mo-Cb Bars & Shapes Bars & Shapes 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 35 [550/240]30 [515/205] Bars & Shapes Bars & Shapes 18Cr-8Ni-N 16Cr-12Ni-2Mo Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form 127] 75/30 [515/205]127] 75/30 [515/205] Forgings Forgings 18Cr-8Ni 16Cr-12Ni-2Mo ≤ ≤ 5 [ 5 [ in [mm] in ≤ ≤ Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 18 18 8.1 1 8.1 1 ASTM 8.1 1 ASTM 8.1 ASTM 8.1 A473 ASTM A473 ASTM A473 302B A473 303 A473 303Se S30215 304 S30300 S30323 304 S30400 S30400 >5 [>127] 75/30 [515/205] 70/30 [485/205] 75/30 [515/205] 75/30 [515/205] Forgings Forgings Forgings Forgings 18Cr-8Ni-2Si 18Cr-8Ni 18Cr-8Ni-S 18Cr-8Ni-Se 888 18 18 8.1 18 8.1 1 ASTM8 8.1 1 ASTM8 8.1 1 ASTM8 8.1 1 A473 ASTM8 8.1 1 A473 ASTM8 8.1 1 A473 ASTM8 8.1 304L 1 A473 ASTM8 8.1 1 305 A473 ASTM8 S30403 8.1 1 316 A473 ASTM/ASME ASTM8 8.1 1 316 A473 S30500 A/SA-479 ASTM/ASME8 8.1 316L 1 A473 S31600 A/SA-479 ASTM/ASME8 8.1 1 317 A473 S31600 A/SA-479 302 ASTM/ASME8 S31603 8.1 >5 [>127] 1 321 A/SA-479 304 ASTM/ASME8 8.1 1 347 S31700 A/SA-479 304H ASTM/ASME8 8.1 S30200 1 348 70/30 [485/205] S32100 A/SA-479 304L 65/25 [450/170] ASTM/ASME8 8.1 S30400 1 304LN S34700 S30409 A/SA-479 ASTM/ASME8 8.1 75/30 [515/205] 1 S34800 A/SA-479 304N S30403 ASTM/ASME8 8.1 S30453 1 A/SA-479 316 ASTM/ASME8 8.1 1 Forgings 316Cb S30451 A/SA-479 65/25 [450/170] Forgings ASTM/ASME 8.1 1 A/SA-479 316H ASTM/ASME 8.1 S31600 75/30 [515/205] Forgings 1 S31640 A/SA-479 316L 75/30 [515/205] ASTM/ASME 8.1 75/30 [515/205] 316LN S31609 A/SA-479 75/30 [515/205] ASTM/ASME 8.1 75/30 [515/205] 75/30 [515/205] A/SA-479 16Cr-12Ni-2Mo 316N S31603 Forgings ASTM/ASME S31653 75/30 [515/205] 70/25 [485/170] 316Ti A/SA-479 75/30 [515/205] 18Cr-8Ni Bars & Shapes Forgings S31651 321 Bars & Shapes 18Cr-11Ni Forgings 80/ S31635 Bars & Shapes 321H Forgings Bars & Shapes 75/30 [515/205] 75/30 16Cr-12Ni-2Mo Bars & Shapes S32100 Forgings S32109 75/ 18Cr-8Ni 18Cr-13Ni-3Mo 18Cr-8Ni 70/25 18Cr-10Ni-Ti 18Cr-8Ni 75/30 Bars & Shapes 18Cr-10Ni-Cb 18Cr-8Ni 18Cr-8Ni-N 80/35 18Cr-10Ni-Cb 75/30 [515/205] 16Cr-12Ni-2Mo 75/30 [515/205] 75/30 [515/205] Bars & Shapes Bars & Shapes Bars & Shapes 16Cr-12Ni-2Mo-Ti 18Cr-10Ni-Ti 18Cr-10Ni-Ti Material Number
141 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Strip 16Cr-12Ni-2Mo Strip 16Cr-12Ni-2Mo eet, & Stripeet, & Strip 18Cr-8Ni-N 18Cr-8Ni-N Sheet, & Strip 18Cr-8Ni Sheet, & Strip 18Cr-8Ni Sheet, & Strip 18Cr-8Ni 170] Plate, Sheet, & 205] Plate, Sheet, & 515/205]515/205]515/205] Seamless Tube Seamless Tube Seamless Tube 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 18Cr-13Ni-3Mo 515/205] Plate, 515/205] Plate, 485/170] Plate, 515/205]550/240] Plate, Sh Plate, Sh [550/220] Bars & Shapes 18Cr-20Ni-5.5Si 35 [540/240] Bars & Shapes 18Cr-15Ni-4Si Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-4798 8.1 1 ASTM8 8.1 1 S32615 ASTM8 8.1 1 S32615 ASTM8 8.1 1 A511 ASTM8 8.1 1 A511 ASTM8 8.1 1 A511 MT 302 ASTM8 8.1 1 A511 MT 304 ASTM8 8.1 1 S30200 A511 MT 304L ASTM8 8.1 1 S30400 A511 MT 316 S30403 ASTM8 8.1 1 A511 MT 316L 80/32 ASTM8 8.1 1 S31600 A511 MT 317 S31603 ASTM8 8.1 1 A554 MT 321 ASTM 8.1 1 S31700 A554 MT 347 ASTM 8.1 1 S32100 A554 MT 302 75/30 [515/205] ASTM 8.1 S34700 A554 MT 304 75/30 [515/205] ASTM 8.1 S30200 A554 MT 304L 75/30 [515/205] ASTM/ASME ASTM S30400 A554 A/SA-666 MT 316 S30403[ 75/30 Seamless Tube A554 MT 316L[ 75/30 Seamless Tube S31600 A554 MT 317 Seamless Tube S31603 302[ 75/30 MT 321 75/30 [515/205] S31700 MT 347 75/30 [515/205] S30200 S32100 18Cr-8Ni 75/30 [515/205] S34700 18Cr-8Ni 75/30 [515/205] 18Cr-8Ni Seamless Tube 70/25 [485/170] Seamless Tube 75/30 [515/205] Tube Welded 70/25 [485/170] Tube Welded 18Cr-10Ni-Ti Tube 75/30 [515/205] Welded 75/30 [ 18Cr-10Ni-Cb 75/30 [515/205] Tube Welded Tube 75/30 [515/205] Welded 18Cr-8Ni Tube Welded 18Cr-8Ni Tube Welded 18Cr-8Ni 16Cr-12Ni-2Mo Tube Welded 16Cr-12Ni-2Mo 18Cr-13Ni-3Mo 18Cr-10Ni-Ti 18Cr-10Ni-Cb 888 18 18 8.1 1 ASTM/ASME 8.1 1 A/SA-479 ASTM/ASME 8.1 1 A/SA-479 ASTM/ASME 8.1 A/SA-479 347 ASTM/ASME 8.1 A/SA-479 347H ASTM/ASME A/SA-479 348 S34700 S34709 348H S30600 S34800 S34809 S30600 75/30 [515/205] 75/30 [515/205] 75/30 [515/205] 75/30 [515/205] 78/ Bars & Shapes Bars & Shapes Bars & Shapes Bars & Shapes 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb 8 1 8.1 ASTM/ASME A/SA-666 304 S30400 75/30 [ 8 1 8.1 ASTM/ASME A/SA-666 304L S30403 70/25 [ 8 1 8.1 ASTM/ASME A/SA-666 316L S31603 70/25 [485/ 888 1 1 8.1 1 ASTM/ASME 8.1 A/SA-666 ASTM/ASME 8.1 A/SA-666 ASTM/ASME 304LN A/SA-666 304N S30453 316 S30451 S31600 75/30 [ 80/35 [ 75/30 [515/ Material Number
142 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Strip 16Cr-12Ni-2Mo-N Wrought Piping FittingsWrought Piping FittingsWrought Piping Fittings 16Cr-12Ni-2Mo Wrought Piping Fittings 18Cr-10Ni-Ti 18Cr-10Ni-Cb 18Cr-13Ni-3Mo 290] Castings 17Cr-9Ni-8Mn-4Si-N 170] Wrought Piping Fittings 18Cr-8Ni 240] Plate, Sheet, & 485/205] Castings 20Cr-11Ni-0.3Se 30 [515/205]25 [485/170]30 [515/205]35 [550/240] Tube Welded Tube Welded Tube Welded Tube Welded 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-688 ASTM/ASME8 8.1 1 A/SA-688 ASTM/ASME8 8.1 1 TP304 A/SA-688 ASTM/ASME8 8.1 1 TP304L A/SA-688 ASTM/ASME TP304LN8 8.1 1 S30400 A/SA-688 S30403 ASTM/ASME8 8.1 TP304N 1 S30453 A/SA-688 ASTM/ASME8 8.1 1 TP316 A/SA-688 S30451 ASTM/ASME8 8.1 1 TP316L A/SA-688 TP316LN8 8.2 1 S31600 S31603 ASTM8 8.1 TP316N 1 S31653 ASTM8 8.1 1 S31651 75/30 [515/205] ASTM8 8.2 1 A743 70/25 [485/170] ASTM 75/30 [515/205]8 8.1 1 A743 ASTM8 8.1 CF10SMnN 1 A743 80/35 [550/240] ASTM8 8.1 J92972 1 Tube Welded A743 CF16F Tube 75/ Welded ASTM8 8.2 1 A743 Tube Welded 70/ ASTM 75/ 8 8.1 CF3 1 A743 J92701 Tube Welded CF3M ASTM8 8.1 1 A743 80/ CF3MN ASTM8 8.1 1 A743 J92500 J92800 18Cr-8Ni ASTM8 8.1 CF8 1 J92804 A743 18Cr-8Ni 18Cr-8Ni-N CF8C ASTM8 8.1 1 A743 CF8M 85/42 [585/ 18Cr-8Ni-N ASTM8 8.1 1 A774 J92600 CG3M J92710 ASTM8 8.1 1 A774 J92900 CG8M ASTM 8.1 1 A774 70/30 [ J92999 ASTM 8.1 304L 1 A774 J93000 ASTM 8.1 316L 70/30 [485/205] A774 70/30 [485/205] 75/37 [515/255] ASTM S30403 8.1 321 A778 ASTM S31603 347 A778 F317L ASTM 70/30 [485/205] A778 S32100 70/30 [485/205] 304L Castings A778 S34700 70/30 [485/205] Castings S31703 Castings 316L A778 75/35 [515/240] S30403 321 75/35 [515/240] S31603 Castings 347 Castings 70/25 [485/ F317L S32100 Castings 70/25 [485/170] 18Cr-12Ni-2Mo 20Cr-11Ni-3Mo-N 18Cr-8Ni Castings S34700 S31703 75/30 [515/205] Castings 75/30 [515/205] 75/30 [515/205] 18Cr-10Ni-Cb 18Cr-8Ni [485/170] 70/25 18Cr-12Ni-2Mo [485/170] 70/25 19Cr-11Ni-4Mo Unannealed Tube Welded 19Cr-10Ni-3Mo [515/205] 75/30 Unannealed Tube Welded [515/205] 75/30 [515/205] 75/30 Unannealed Tube Welded 18Cr-8Ni 16Cr-12Ni-2Mo Unannealed Tube Welded Unannealed Tube Welded 18Cr-10Ni-Ti 18Cr-13Ni-3Mo 18Cr-10Ni-Cb 8 1 8.1 ASTM/ASME A/SA-666 316N S31651 80/35 [550/ Material Number
143 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Cold Worked Welded Pipe Welded Worked Cold Pipe Welded Worked Cold 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 205]240] Pipe Welded Worked Cold 205] Pipe Welded Worked Cold 205] Pipe Welded Worked Cold 18Cr-8Ni-N 170] Pipe Welded Worked Cold 18Cr-8Ni-N 16Cr-12Ni-2Mo Pipe Welded Worked Cold 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 515/205]515/205] Pipe Welded Worked Cold 485/170] Pipe Welded Worked Cold Pipe Welded Worked Cold 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 30 [515/205]30 [515/205]25 [485/170]30 [515/205] Pipe Welded 35 [550/240] Pipe Welded 30 [515/205] Pipe Welded 30 [515/205] Pipe Welded 16Cr-12Ni-2Mo Pipe Welded 16Cr-12Ni-2Mo Pipe Welded 16Cr-12Ni-2Mo Pipe Welded 16Cr-12Ni-2Mo-N 16Cr-12Ni-2Mo-N 18Cr-13Ni-3Mo 18Cr-13Ni-3Mo Minimum Minimum Tensile/Yield Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 8 1 8.1 ASTM/ASME A/SA-814 TP316N S31651 80/35 [550/240] 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-813 ASTM/ASME8 8.1 1 A/SA-813 ASTM/ASME8 8.1 TP316H 1 A/SA-813 ASTM/ASME8 8.1 1 TP316L A/SA-813 S31609 ASTM/ASME TP316LN8 8.1 1 A/SA-813 S31603 ASTM/ASME8 8.1 TP316N 1 S31653 A/SA-813 ASTM/ASME8 8.1 1 TP317 A/SA-813 S31651 ASTM/ASME8 8.1 1 TP317L A/SA-813 ASTM/ASME8 8.1 1 S31700 TP321 A/SA-813 S31703 ASTM/ASME8 8.1 TP321H 1 A/SA-813 ASTM/ASME8 8.1 1 S32100 75/ TP347 A/SA-813 S32109 ASTM/ASME8 8.1 TP347H 1 70/ A/SA-813 ASTM/ASME 75/ 8 8.1 1 S34700 TP348 A/SA-813 S34709 ASTM/ASME8 8.1 TP348H 1 80/ A/SA-814 ASTM/ASME TPXM-158 8.1 1 S34800 A/SA-814 S34809 75/ ASTM/ASME8 8.1 1 S38100 TP304 75/ A/SA-814 ASTM/ASME8 8.1 TP304H 1 A/SA-814 75/30 [515/205] ASTM/ASME 8.1 1 S30400 TP304L 75/30 [515/205] A/SA-814 S30409 ASTM/ASME TP304LN 8.1 1 A/SA-814 S30403 75/30 [515/205] ASTM/ASME 8.1 TP304N S30453 75/30 [515/205] A/SA-814 ASTM/ASME 8.1 Pipe Welded TP316 A/SA-814 S30451 Pipe 75/30 [515/205] Welded ASTM/ASME TP316H 75/30 [515/205] A/SA-814 75/30 [515/205] S31600 TP316L Pipe Welded S31609 Pipe Welded TP316LN S31603 75/30 [ S31653 Pipe 75/30 [ Welded 18Cr-10Ni-Ti Pipe Welded 18Cr-10Ni-Ti Pipe Welded 70/25 [ 75/30 [515/ 18Cr-10Ni-Cb 18Cr-10Ni-Cb 80/35 [550/ 18Cr-10Ni-Cb 18Cr-10Ni-Cb 75/30 [515/ 18Cr-18Ni-2Si 75/30 [515/ 70/25 [485/ 75/30 [515/205] 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-813 ASTM/ASME 8.1 1 A/SA-813 ASTM/ASME 8.1 1 TP304 A/SA-813 ASTM/ASME 8.1 TP304H A/SA-813 ASTM/ASME 8.1 S30400 TP304L A/SA-813 S30409 ASTM/ASME TP304LN A/SA-813 S30403 TP304N S30453 TP316 S30451 S31600 75/30 [515/205] 75/30 [515/205] 70/25 [485/170] 75/30 [515/205] Pipe 80/35 [550/240] Welded Pipe Welded 75/ Pipe Welded Pipe Welded Pipe Welded 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni 18Cr-8Ni-N 18Cr-8Ni-N Material Number
144 AWS B2.1/B2.1M-BMG:2014 Nominal Composition ate, Sheet, & Stripate, Sheet, & Stripate, Sheet, & Strip 20Cr-10Ni 23Cr-12Ni 25Cr-20Ni 205]205] Pipe Welded Worked Cold 205] Pipe Welded Worked Cold 205] 18Cr-13Ni-3Mo Pipe Welded Worked Cold 205] 18Cr-13Ni-3Mo Pipe Welded Worked Cold 205] Pipe Welded Worked Cold 18Cr-10Ni-Ti 205] Pipe Welded Worked Cold 18Cr-10Ni-Ti 205] Pipe 18Cr-10Ni-Cb Welded Worked Cold 205] Pipe 18Cr-10Ni-Cb Welded Worked Cold Pipe 18Cr-10Ni-Cb Welded Worked Cold 18Cr-10Ni-Cb 18Cr-18Ni-2Si Minimum Minimum Tensile/Yield 70/30 [485/205]70/30 [485/205]65/25 [450/170]80/35 [550/240] Forgings Forgings Forgings Forgings 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo 16Cr-12Ni-2Mo-N Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 8 1 8.1 ASTM/ASME A/SA-814 TP317 S31700 75/30 [515/ 888 18 18 8.1 1 ASTM/ASME8 8.1 1 A/SA-814 ASTM/ASME8 8.1 1 A/SA-814 ASTM/ASME8 8.1 1 TP317L A/SA-814 ASTM/ASME8 8.1 1 TP321 A/SA-814 S31703 ASTM/ASME8 8.1 TP321H 1 A/SA-814 ASTM/ASME8 8.1 1 S32100 TP347 A/SA-814 S32109 ASTM/ASME8 8.1 TP347H 1 A/SA-814 ASTM/ASME8 8.1 1 S34700 TP348 A/SA-814 S34709 ASTM/ASME8 8.1 TP348H 1 A/SA-965 ASTM/ASME TPXM-158 8.1 1 S34800 A/SA-965 S34809 ASTM/ASME8 8.1 1 S38100 75/30 [515/ A/SA-965 F304 ASTM/ASME8 8.1 1 F304H A/SA-965 75/30 [515/ ASTM/ASME8 8.1 1 75/30 [515/ F304L A/SA-965 S30400 ASTM/ASME8 8.1 S30409 F304LN 1 A/SA-965 75/30 [515/ ASTM/ASME8 8.1 1 S30403 75/30 [515/ F304N A/SA-965 S30453 ASTM/ASME8 8.1 1 A/SA-965 F316 75/30 [515/ ASTM/ASME8 8.1 S30451 1 75/30 [515/ F316H A/SA-965 75/30 [515/ ASTM/ASME8 8.1 1 F316L A/SA-965 S31600 ASTM/ASME8 8.1 S31609 F316LN 1 A/SA-965 ASTM/ASME8 8.1 1 S31603 70/30 [485/205] F316N A/SA-965 S31653 70/30 [485/205] ASTM/ASME8 8.1 1 A/SA-965 F321 65/25 [450/170] ASTM/ASME 8.1 S31651 1 70/30 [485/205] F321H A/SA-965 ASTM/ASME 8.1 2 A/SA-965 S32100 F347 80/35 [550/240] ASTM/ASME 8.1 S32109 Forgings F347H A/SA-965 Forgings ASTM/ASME 8.2 A/SA-965 S34700 F348 Forgings S34709 F348H Forgings ASTM 70/30 [485/205] S34800 F46 Forgings S34809 A167 18Cr-8Ni S30600 18Cr-8Ni 70/30 [485/205] 70/30 [485/205] 18Cr-8Ni 18Cr-8Ni-N Forgings 308 70/30 [485/205] 18Cr-8Ni-N 70/30 [485/205] 70/30 [485/205] Forgings S30800 70/30 [485/205] Forgings 16Cr-12Ni-2Mo-N Forgings 78/32 [540/220] Forgings Forgings Forgings 18Cr-10Ni-Ti 18Cr-10Ni-Ti Forgings 18Cr-10Ni-Cb 75/30 [515/205] 18Cr-10Ni-Cb 18Cr-10Ni-Cb 18Cr-10Ni-Cb Pl 18Cr-15Ni-4Si 88 2 2 8.2 8.2 ASTM ASTM A167 A167 309 310 S30900 S31000 75/30 [515/205] 75/30 [515/205] Pl Pl Material Number
145 AWS B2.1/B2.1M-BMG:2014 Nominal Composition eet, & Strip 23Cr-12Ni-Cb eet, & Strip 25Cr-22Ni-2Mo-N eet, & Strip 25Cr-20Ni-Cb eet, & Strip 21Cr-11Ni-N Sheet, & Strip 23Cr-12Ni Sheet, & Strip 23Cr-12Ni Sheet, & Strip 25Cr-20Ni Sheet, & Strip 25Cr-20Ni Sheet, & Strip 25Cr-22Ni-2Mo-N 205] Plate, Sheet, & Strip 23Cr-12Ni-Cb 205] Plate, Sheet, & Strip 25Cr-20Ni-Cb 515/205] Plate, 515/205]515/205] Plate, Sh Plate, 515/205] Plate, 515/205] Plate, 515/205] Plate, Sh 600/310] Plate, Sh [540/255] Plate, Sh 30 [515/205]45 [600/310] Seamless Tube Seamless Tube 25Cr-20Ni 21Cr-11Ni-N Minimum Minimum Tensile/Yield 78/37 [540/255]75/30 [515/205] Forgings75/30 [515/205]75/30 [515/205]75/30 [515/205] Seamless Tube 25Cr-22Ni-2Mo-N 75/30 [515/205] Seamless Tube75/30 [515/205] Seamless Tube75/30 [515/205] Seamless Tube 23Cr-12Ni-Cb Seamless Tube Seamless Tube 23Cr-12Ni 23Cr-12Ni-Cb Seamless Tube 23Cr-12Ni 25Cr-20Ni-Cb 25Cr-20Ni 25Cr-20Ni-Cb 75/30 [515/205] Seamless Tube 25Cr-20Ni 87/45 [600/310] Tube Welded 21Cr-11Ni-N Strength, ksi [MPa] Product Form 6] 78/37 [540/255] Seamless Tube 25Cr-22Ni-2Mo-N 6] 84/39 [580/270] Seamless Tube 25Cr-22Ni-2Mo-N 6] 84/39 [580/270] Plate, ≤ ≤ 5 [>127] 70/30 [485/205] Forgings 25Cr-20Ni 0.25 [ 0.25 [ in [mm] in Thickness ≤ ≤ or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 28 28 8.2 2 ASTM/ASME8 8.2 2 A/SA-182 ASTM/ASME8 8.2 2 A/SA-182 F310MoLN ASTM/ASME8 8.2 2 A/SA-213 S31050 ASTM/ASME8 8.2 2 A/SA-213 F45 ASTM/ASME8 8.2 2 A/SA-213 310 ASTM/ASME8 8.2 2 S30815 A/SA-213 ASTM/ASME S308158 8.2 TP309Cb 2 A/SA-213 ASTM/ASME S308158 8.2 S31000 TP309H 2 S30940 A/SA-213 TP309HCb ASTM/ASME 8.2 2 A/SA-213 S30909 S30941 ASTM/ASME 8.2 2 TP309S A/SA-213 ASTM/ASME 8.2 TP310Cb A/SA-213 S30908 ASTM/ASME 8.2 TP310H S31040 A/SA-213 TP310HCb ASTM/ASME TP310MoLN A/SA-213 87/45 [600/310] S31009 S31041 S31050 TP310MoLN 87/ 75/ S31050 >0.25 [> Forgings 21Cr-11Ni-N 888 2 2 8.1 2 ASTM/ASME 8.2 A/SA-182 ASTM/ASME 8.2 A/SA-182 ASTM/ASME A/SA-182 F10 F310 F310 S33100 S31000 S31000 > 80/30 [550/205] 75/30 [515/205] Forgings Forgings 20Ni-8Cr 25Cr-20Ni 888 2 2 8.2 2 ASTM/ASME 8.2 A/SA-213 ASTM/ASME 8.2 A/SA-240 ASTM/ASME TP310S A/SA-240 309Cb S31008 309H S30940 S30909 75/30 [515/ 75/30 [ 88 2 2 8.2 ASTM/ASME 8.2 A/SA-240 ASTM/ASME A/SA-240 309HCb 309S S30941 S30908 75/30 [ 75/30 [ 88 2 2 8.2 ASTM/ASME 8.2 A/SA-240 ASTM/ASME A/SA-240 310Cb 310H S31040 S31009 75/30 [515/ 75/30 [ 8 2 8.2 ASTM/ASME A/SA-240 310MoLN S31050 >0.25 [>6] 78/37 8 2 8.2 ASTM/ASME A/SA-240 310S S31008 75/30 [ 88 2 2 8.2 ASTM/ASME 8.2 A/SA-240 ASTM/ASME A/SA-240 310HCb 310MoLN S31041 S31050 75/30 [ 88 2 2 8.2 ASTM/ASME 8.2 A/SA-240 ASTM/ASME A/SA-249 S30815 S30815 S30815 S30815 87/45 [ Material Number
146 AWS B2.1/B2.1M-BMG:2014 Nominal Composition 600/310]Pipe Seamless & Welded 21Cr-11Ni-N [515/205][515/205]Pipe Seamless & Welded [515/205]Pipe Seamless & Welded [515/205]Pipe Seamless & Welded 23Cr-12Ni-Cb [515/205]Pipe Seamless & Welded [515/205] 23Cr-12Ni Pipe Seamless & Welded 23Cr-12Ni-Cb [515/205]Pipe Seamless & Welded 23Cr-12Ni Pipe Seamless & Welded 25Cr-20Ni-Cb 25Cr-20Ni 25Cr-20Ni-Cb [515/205]Pipe Seamless & Welded 25Cr-20Ni 37 [540/255]37 Pipe Seamless & Welded 25Cr-22Ni-2Mo-N Minimum Minimum Tensile/Yield 80/40 [550/275] Castings 25Cr-8Ni-N Strength, ksi [MPa] Product Form 6] 78/37 [540/255] Tube Welded 25Cr-22Ni-2Mo-N 6] 84/39 [580/270] Tube Welded 25Cr-22Ni-2Mo-N 6][580/270] 84/39 Pipe Seamless & Welded 25Cr-22Ni-2Mo-N ≤ ≤ 0.25 [ 0.25 [ in [mm] in Thickness ≤ ≤ or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 28 28 8.2 2 ASTM/ASME8 8.2 2 A/SA-249 ASTM/ASME8 8.2 2 A/SA-249 ASTM/ASME8 8.2 2 TP309 A/SA-249 ASTM/ASME8 8.2 TP309Cb 2 A/SA-249 ASTM/ASME 8.2 TP309H 2 S30900 S30940 A/SA-249 TP309HCb ASTM/ASME 8.2 2 A/SA-249 S30909 S30941 ASTM/ASME 8.2 TP309S A/SA-249 ASTM/ASME 8.2 TP310Cb A/SA-249 S30908 ASTM/ASME TP310H S31040 A/SA-249 TP310HCb TP310MoLN S31009 S31041 S31050 75/30 [515/205] 75/30 [515/205] 75/30 [515/205] 75/30 [515/205] Tube Welded Tube 75/30 [515/205] Welded 75/30 [515/205] Tube Welded Tube Welded 75/30 [515/205] 75/30 [515/205] Tube Welded 23Cr-12Ni-Cb Tube Welded 23Cr-12Ni Tube 23Cr-12Ni-Cb Welded Tube Welded 23Cr-12Ni 23Cr-12Ni 25Cr-20Ni-Cb 25Cr-20Ni-Cb 25Cr-20Ni 888 28 28 8.2 2 ASTM/ASME8 8.2 2 A/SA-249 ASTM/ASME8 8.2 2 TP310MoLN A/SA-2498 8.2 2 S31050 ASTM8 8.2 2 TP310S >0.25 [> ASTM8 8.2 2 S31008 ASTM8 8.2 2 A297 ASTM8 8.2 2 A297 ASTM/ASME ASTM8 8.2 2 A297 A/SA-312 ASTM/ASME8 8.2 2 HE A297 A/SA-312 ASTM/ASME8 8.2 2 S30815 HF A297 A/SA-312 ASTM/ASME8 8.2 TP309Cb 2 HH A/SA-312 J93403 ASTM/ASME S30815 8.2 TP309H 2 S30940 HI 75/30 [515/205] A/SA-312 J92603 TP309HCb ASTM/ASME 8.2 2 HK J93503 A/SA-312 S30909 S30941 ASTM/ASME 8.2 TP309S A/SA-312 J94003 ASTM/ASME 8.2 TP310Cb J94224 A/SA-312 S30908 Tube ASTM/ASME Welded TP310H S31040 A/SA-312 TP310HCb TP310MoLN S31009 S31041 S31050 85/40 [585/275] 87/45 [ 75/30 70/35 [485/240] 25Cr-20Ni 75/35 [515/240] 75/30 75/30 70/35 [485/240] 65/35 [450/240] Castings 75/30 75/30 Castings Castings 75/30 75/30 Castings 28Cr-10Ni-2Mn-2Si Castings 21Cr-10Ni-2Mn-2Si 26Cr-13Ni-2Mn-2Si 28Cr-16Ni-2Mn-2Si 26Cr-20Ni-2Mn-2Si 888 28 2 8.2 2 ASTM/ASME 8.2 2 A/SA-312 ASTM/ASME 8.2 TP310MoLN A/SA-312 ASTM/ASME 8.2 S31050 A/SA-336 ASTM/ASME TP310S A/SA-351 >0.25 [>6] F310 S31008 CE20N 78/ S31000 J92802 75/30 75/30 [515/205] Forgings 25Cr-20Ni Material Number
147 AWS B2.1/B2.1M-BMG:2014 Nominal Composition ng Fittingsng Fittingsng Fittings 23Cr-12Ni 23Cr-12Ni 25Cr-20Ni 550/275]485/205]485/205]Pipe Cast Centrifugal 450/195]Pipe Cast Centrifugal 450/195]Pipe Cast Centrifugal Pipe Cast Centrifugal 25Cr-8Ni-N Pipe Cast Centrifugal 25Cr-12Ni 25Cr-12Ni 25Cr-12Ni 25Cr-20Ni [450/240][425/240][515/205] Castings Castings Pipe Fusion Welded [515/205][600/310] 25Cr-20Ni-0.5Mo 25Cr-20Ni-0.5Mo Pipe Fusion Welded 23Cr-12Ni Pipe Fusion Welded 25Cr-20Ni 21Cr-11Ni-N 30 [515/205]30 [515/205] Wrought Pipi 30 [515/205] Wrought Pipi Wrought Pipi Minimum Minimum Tensile/Yield 87/45 [600/310] Pipe Welded 21Cr-11Ni-N Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS 934019340294202 70/30 [485/205] 70/30 [485/205] 65/28 [450/195] Castings Castings Castings 25Cr-12Ni 25Cr-12Ni 25Cr-20Ni Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 8 2 8.2 ASTM/ASME A/SA-351 CH10 J 888 28 28 8.2 2 ASTM/ASME8 8.2 2 A/SA-351 ASTM/ASME8 8.2 2 A/SA-351 ASTM/ASME8 8.2 2 CH20 A/SA-351 ASTM/ASME8 8.2 2 A/SA-351 CH8 ASTM/ASME8 8.2 2 J CK20 A/SA-351 ASTM/ASME8 8.2 2 HK30 A/SA-358 J93400 ASTM/ASME8 8.2 2 J HK40 A/SA-358 ASTM/ASME8 8.2 2 J94203 A/SA-358 309 ASTM/ASME8 8.2 2 J94204 309Cb A/SA-358 ASTM/ASME8 8.2 2 A/SA-358 309S ASTM/ASME8 8.2 S30900 2 S30940 A/SA-358 310 ASTM/ASME8 8.2 2 310Cb A/SA-358 S30908 ASTM/ASME8 8.2 2 65/28 [450/195] A/SA-403 310S ASTM/ASME8 S31000 8.2 2 S31040 S30815 A/SA-403 ASTM/ASME8 8.2 65/35 2 WP309 A/SA-403 S31008 ASTM/ASME S308158 8.2 62/35 2 WP310 A/SA-409 ASTM/ASME S309008 8.2 WP310S 2 A/SA-409 Castings 75/30 [515/205] 75/30 [515/205] ASTM/ASME S310008 8.2 2 S30815 A/SA-409 S31008 ASTM/ASME8 8.2 TP309Cb 2 75/30 A/SA-409 ASTM/ASME S30815 8 8.2 Pipe Fusion Welded 2 TP309S Pipe Fusion Welded S30940 A/SA-409 75/30 [515/205] 75/30 [515/205] ASTM/ASME8 8.2 TP310Cb 2 A/SA-451 S30908 ASTM/ASME8 8.2 2 TP310S 75/30 S31040 A/SA-451 87/45 25Cr-12Ni ASTM/ASME8 8.2 Pipe CPE20N Fusion Welded 2 23Cr-12Ni-Cb Pipe Fusion Welded A/SA-451 23Cr-12Ni 75/ S31008 ASTM/ASME 8.2 2 CPH10 A/SA-451 J92802 75/ ASTM/ASME 8.2 2 75/ CPH20 A/SA-451 8.2 J93402 25Cr-20Ni-Cb CPH8 23Cr-12Ni ASTM 8.2 J93402 75/30 [515/205] CPK20 ASTM J93400 75/30 [515/205] ASTM J94202 75/30 [515/205] A473 A473 75/30 [515/205] Pipe Welded A473 80/40 [ Pipe Welded 308 Pipe Welded 70/30 [ 309 70/30 [ Pipe Welded 309S S30800 23Cr-12Ni-Cb 65/28 [ S30900 65/28 [ S30908 23Cr-12Ni 25Cr-20Ni-Cb 25Cr-20Ni 75/30 [515/205] 75/30 [515/205] 75/30 [515/205] Forgings Forgings Forgings 20Cr-10Ni 23Cr-12Ni 23Cr-12Ni Material Number
148 AWS B2.1/B2.1M-BMG:2014 Nominal Composition 310] Pipe Welded Worked Cold 21Cr-11Ni-N 515/205]515/205] Pipe Welded Worked Cold 515/205] Pipe Welded Worked Cold Pipe 23Cr-12Ni-Cb Welded Worked Cold 23Cr-12Ni 25Cr-20Ni-Cb 45 [600/310] Bars & Shapes 21Cr-11Ni-N Minimum Minimum Tensile/Yield 87/45 [600/310] Pipe Welded 21Cr-11Ni-N Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 28 28 8.2 28 8.2 2 ASTM8 8.2 2 ASTM8 8.2 2 ASTM8 8.2 2 A511 ASTM8 8.2 2 A511 ASTM8 8.2 2 A554 MT 309S ASTM8 8.2 2 A554 MT 310S S30908 ASTM8 8.2 2 A554 MT 309S S31008 MT 309S-Cb ASTM8 8.2 2 A743 S30940 S30908 ASTM8 8.2 2 A743 MT 310S ASTM8 8.2 2 A743 S31008 ASTM/ASME ASTM CE308 8.2 2 A743 A/SA-813 ASTM/ASME CF208 8.2 2 A743 A/SA-813 ASTM/ASME CG12 J934238 8.2 2 S30815 A743 75/30 [515/205] A/SA-813 ASTM/ASME CH10 J926028 8.2 TP309Cb 2 75/30 [515/205] A/SA-813 J93001 ASTM/ASME S30815 CH20 8.2 2 TP309S S30940 75/30 [515/205] 75/30 [515/205] A/SA-813 CN3M J93401 ASTM/ASME 8.2 TP310Cb 2 A/SA-814 Seamless Tube S30908 J93402 ASTM/ASME 8.2 TP310S S31040 75/30 [515/205] A/SA-814 J94652 Seamless Tube ASTM/ASME 8.2 S30815 A/SA-814 S31008 Tube Tube ASTM/ASME Welded Welded TP309Cb A/SA-814 80/40 [550/275] S30815 TP309S S30940 70/30 [485/205] 23Cr-12Ni Tube Welded TP310Cb 70/28 [485/195] S30908 25Cr-20Ni 75/30 [515/205] S31040 70/30 [485/205] 23Cr-12Ni-Cb 23Cr-12Ni 75/30 [515/205] 70/30 [485/205] Castings 75/30 [515/205] 63/25 [435/170] Castings 25Cr-20Ni 75/30 [515/205] Pipe Welded Castings 87/45 [600/ Castings Pipe Welded 75/30 [ Pipe Welded 29Cr-9Ni-2Mn-2Si Castings Castings 75/30 [ Pipe Welded 75/30 [ 23Cr-12Ni-Cb 20Cr-10Ni 22Cr-12Ni 23Cr-12Ni 25Cr-20Ni-Cb 25Cr-12Ni 25Ni-21Cr-5Mo 25Cr-12Ni 25Cr-20Ni 888 28 28 8.2 28 8.2 2 ASTM8 8.2 2 ASTM8 8.2 2 ASTM8 8.2 2 A473 ASTM/ASME ASTM 8.2 2 A473 A/SA-479 ASTM/ASME 8.2 2 A473 A/SA-479 ASTM/ASME 8.2 310 A473 309Cb A/SA-479 ASTM/ASME 8.2 310S A/SA-479 309S ASTM/ASME S30940 314 S31000 310Cb A/SA-479 S30815 S31008 S30908 310S S31040 S30815 S30815 S31400 S31008 S30815 75/30 [515/205] 75/30 [515/205] 75/30 [515/205] 75/30 [515/205] 75/30 [515/205] 87/45 [600/310] 75/30 [515/205] Bars & Shapes 75/30 [515/205] 87/ Forgings Bars & Shapes Forgings Bars & Shapes Forgings Forgings Bars & Shapes 23Cr-12Ni-Cb 23Cr-12Ni 25Cr-20Ni-Cb 25Cr-20Ni 25Cr-20Ni 25Cr-20Ni 21Cr-11Ni-N 25Cr-21Ni-S Material Number
149 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Strip 18Cr-8Ni-4Si-N & Strip 18Cr-3Ni-12Mn Plate, Sheet, & Strip 16Cr-9Mn-2Ni-N amless & Welded Tubeamless & Welded Tubeamless & Welded Tubeamless & Welded 20Cr-6Ni-9Mn 21Cr-6Ni-9Mn 18Cr-18Ni-2Si Seamless & Welded TubeSeamless & Welded 22Cr-13Ni-5Mn 380] Plate, Sheet, 260]310]310] Plate, Sheet, & Strip260] Plate, Sheet, & Strip345] Plate, Sheet, & Strip 17Cr-4Ni-6Mn Plate, Sheet, & Strip 17Cr-4Ni-6Mn Plate, Sheet, & 16Cr-4Ni-6Mn 18Cr-5Ni-9Mn 690/415]690/415] Sheet & Strip Sheet & Strip 19Cr-8Mn-6Ni-Mo-N 19Cr-8Mn-6Ni-Mo-N 515/205] Pipe Welded Worked Cold 25Cr-20Ni [725/415] Sheet & Strip 22Cr-13Ni-5Mn [690/380] Seamless Tube 22Cr-13Ni-5Mn 38 [655/260]45 [620/310]43 [655/295] Seamless Tube Seamless Tube Seamless Tube 17Cr-4Ni-6Mn 18Cr-5Ni-9Mn 25Cr-20Ni-Cb-N Minimum Minimum Tensile/Yield 90/50 [620/345]90/50 [620/345] Plate Plate95/38 [655/260]90/38 [620/260] 19Cr-8Mn-6Ni-Mo-N Tube Welded 19Cr-8Mn-6Ni-Mo-N Tube Welded 17Cr-4Ni-6Mn 18Cr-5Ni-9Mn 100/55 [690/380]100/55 [690/380] Plate100/55 [690/380] Tube Welded Tube Welded 22Cr-13Ni-5Mn 22Cr-13Ni-5Mn 18Cr-3Ni-12Mn Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 38 38 8.3 3 ASTM/ASME8 8.3 3 A/SA-240 ASTM/ASME8 8.3 3 A/SA-240 ASTM/ASME8 8.3 3 XM-17 A/SA-240 ASTM/ASME8 8.3 3 XM-17 A/SA-240 ASTM/ASME8 8.3 S21600 3 XM-18 A/SA-240 ASTM/ASME8 S21600 8.3 3 XM-18 A/SA-240 ASTM/ASME8 8.3 S21603 3 XM-19 A/SA-240 ASTM/ASME8 8.3 S21603 3 XM-19 A/SA-249 ASTM/ASME8 S20910 8.3 3 XM-29 A/SA-249 ASTM/ASME8 8.3 S20910 3 TP 201 A/SA-249 ASTM/ASME 8.3 S24000 3 TP 202 A/SA-249 TP XM-19 8.3 S20100 3 100/60 [ TP XM-29 ASTM 8.3 S20200 S20910 ASTM 8.3 S24000 100/60 [ ASTM A269 105/60 ASTM A269 A269 TPXM-10 100/55 [690/ A269 TPXM-11 S21900 TPXM-15 S21904 TPXM-19 S38100 S20910 90/50 [620/345] 90/50 [620/345] Se 90/50 [620/345] Se 100/55 [690/380] Se 8 2 8.2 ASTM/ASME A/SA-814 TP310S S31008 75/30 [ 888 28 38 8.2 3 ASTM/ASME8 8.3 3 A/SA-965 ASTM/ASME8 8.3 3 A/SA-182 ASTM/ASME8 8.3 3 A/SA-182 F310 ASTM/ASME8 8.3 FXM-11 3 A/SA-213 ASTM/ASME8 8.2 FXM-19 3 A/SA-213 S31000 S21904 ASTM/ASME8 8.3 3 TP201 A/SA-213 S20910 ASTM/ASME8 8.3 3 TP202 TP310HCbN A/SA-213 ASTM/ASME8 8.3 3 S20100 S31042 A/SA-240 ASTM/ASME 8.3 3 S20200 XM-19 A/SA-240 ASTM/ASME 8.3 3 A/SA-240 ASTM/ASME 8.3 — S20910 201-1 A/SA-240 ASTM/ASME 8.1 75/30 [515/205] 90/50 [620/345] 201-2 A/SA-240 ASTM/ASME 100/55 [690/380] S20400 201LN S20100 A/SA-240 S20100 202 95/ 95/ S20153 S21800 90/ Forgings Forgings S21800 S20200 Forgings 100/55 95/48 [655/330] 75/38 [515/ 21Cr-6Ni-9Mn 95/45 [655/ 22Cr-13Ni-5Mn 25Cr-20Ni 95/45 [655/ 95/50 [655/ 90/38 [620/ Material Number
150 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Fittings 22Cr-13Ni-5Mn Seamless & Welded TubeSeamless & Welded 18Cr-3Ni-12Mn 380] Pipe Welded Worked Cold 22Cr-13Ni-5Mn 260]310]345] Plate, Sheet, & Strip Plate, Sheet, & Strip Plate, Sheet, & Strip 17Cr-4Ni-6Mn 17Cr-4Ni-6Mn 345] 21Cr-6Ni-9Mn Pipe Welded Worked Cold 21Cr-6Ni-9Mn 690/380]690/380]Pipe Seamless & Welded Pipe Seamless & Welded 22Cr-13Ni-5Mn 18Cr-3Ni-12Mn 690/380]690/380] Pipe Fusion Welded Pipe Fusion Welded 22Cr-13Ni-5Mn 18Cr-3Ni-12Mn [690/380] Wrought Piping [690/380][690/380] Bars & Shapes Bars & Shapes 22Cr-13Ni-5Mn 18Cr-3Ni-12Mn [620/345]Pipe Seamless & Welded 21Cr-6Ni-9Mn [655/345][620/345][620/345] Bars & Shapes Bars & Shapes Bars & Shapes 18Cr-8Ni-4Si-N 19Cr-8Mn-6Ni-Mo-N 19Cr-8Mn-6Ni-Mo-N 55 [690/380]55 [690/380] Pipe Welded Pipe Welded 22Cr-13Ni-5Mn 18Cr-3Ni-12Mn 50 [620/345] Bars & Shapes 21Cr-6Ni-9Mn Minimum Minimum Tensile/Yield 85/42 [585/290] Castings 22Cr-12Ni-5Mn Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 888 38 38 8.3 3 ASTM/ASME8 8.3 3 A/SA-312 ASTM/ASME8 8.3 3 A/SA-312 TP XM-11 ASTM/ASME8 8.3 3 A/SA-312 TP XM-19 ASTM/ASME8 8.3 S21904 3 A/SA-336 TP XM-29 ASTM/ASME8 8.3 S20910 3 A/SA-336 ASTM/ASME8 8.3 S24000 FXM-11 3 A/SA-351 ASTM/ASME8 8.3 FXM-19 3 A/SA-358 S21904 CG6MMN ASTM/ASME8 8.3 3 A/SA-358 S20910 ASTM/ASME8 8.3 J93790 3 XM-19 A/SA-4038 8.3 3 XM-29 90/50 WPXM-19 ASTM8 8.3 S20910 3[ 100/55 ASTM S209108 8.3 S24000 3[ 100/55 ASTM8 8.1 3 A473 ASTM/ASME ASTM8 8.3 3 90/50 [620/345] A473 A/SA-479 ASTM/ASME8 8.3 100/55 [690/380] 3 A473 A/SA-479 ASTM/ASME8 8.3 3 201 S21800 A473 A/SA-479 ASTM/ASME8 8.3 3 202 XM-11 100/55 [ A/SA-479 XM-10 ASTM/ASME S218008 8.3 3 XM-17 Forgings S20100 100/55 100/55 [ A/SA-479 XM-11 ASTM/ASME8 S21904 8.3 Forgings 3 XM-18 S21900 S20200 A/SA-479 ASTM/ASME8 8.3 S21600 3 XM-19 S21904 A/SA-666 ASTM/ASME8 8.3 S21603 3 XM-29 A/SA-666 ASTM/ASME8 S20910 8.3 3 201-1 A/SA-666 21Cr-6Ni-9Mn ASTM/ASME8 8.3 S24000 3 22Cr-13Ni-5Mn 201-2 A/SA-688 ASTM/ASME 8.3 3 XM-11 S20100 A/SA-813 95/50 ASTM/ASME 8.3 75/30 [515/205] 3 XM-29 S20100 A/SA-813 90/ ASTM/ASME TPXM-11 8.3 S21904 90/50 [620/345] 90/45 [620/310] A/SA-813 90/50 ASTM/ASME TPXM-19 8.3 S24000 90/50 [620/345] S21904 A/SA-814 90/50 ASTM/ASME TPXM-29 S20910 100/55 A/SA-814 TPXM-11 Forgings S24000 100/55 TPXM-19 Forgings Forgings S21904 75/38 [515/ Forgings S20910 95/45 [655/ 90/50 [620/ 100/55 [690/380] 17Cr-4Ni-6Mn 90/50 [620/345] 20Cr-6Ni-9Mn 18Cr-5Ni-9Mn 100/ 21Cr-6Ni-9Mn 100/ Tube Welded 90/50 [620/ Pipe Welded 100/55 [690/ 18Cr-3Ni-12Mn 21Cr-6Ni-9Mn 8 3 8.3 ASTM A269 TPXM-29 S24000 100/55 [690/380] Material Number
151 AWS B2.1/B2.1M-BMG:2014 Nominal Composition Strip 19Cr-15.5Ni-4Mo Strip 19Cr-15Ni-4Mo ate, Sheet, & Strip 23Cr-25Ni-5.5Mo-N Fusion Welded PipeFusion Welded 23Cr-25Ni-5.5Mo-N amless & Welded Pipe amless & Welded 23Cr-25Ni-5.5Mo-N Plate, Sheet, & Strip 24Cr-17Ni-6Mn-4.5Mo-N Seamless & Welded Pipe Seamless & Welded 24Cr-17Ni-6Mn-4.5Mo-N 380] Pipe Welded Worked Cold 18Cr-3Ni-12Mn 415] Seamless Tube 24Cr-17Ni-6Mn-4.5Mo-N 240]Pipe Seamless & Welded 19Cr-15.5Ni-4Mo 240] Plate, Sheet, & 205] Plate, Sheet, & 515/205]Pipe Seamless & Welded 19Cr-15Ni-4Mo [690/310] Sheet & Strip 20Cr-18Ni-6Mo [650/310] Tube Welded Fusion 20Cr-18Ni-6Mo [550/240] Tube Welded 19Cr-15.5Ni-4Mo 45 [655/310]45 Pipe Seamless & Welded 20Cr-18Ni-6Mo 30 [515/205] Tube Welded 19Cr-15Ni-4Mo 30 [515/205]35 [550/240] Seamless Tube Seamless Tube 19Cr-15Ni-4Mo 19Cr-15.5Ni-4Mo Minimum Minimum Tensile/Yield 80/38 [550/260] Castings 20Cr-18Ni-6Mo Strength, ksi [MPa] Product Form 5] 95/45 [655/310] Tube Welded 20Cr-18Ni-6Mo 5][675/310] 98/45 Pipe Seamless & Welded 20Cr-18Ni-6Mo 5] 98/45 [675/310] Tube Welded 20Cr-18Ni-6Mo ≤ ≤ in [mm] in Thickness 0.1875 [ 0.1875 [ or Diameter or Diameter Limitations, ≤ ≤ .2 (Continued) (Continued) 4 95/45 [655/310] Plate 20Cr-18Ni-6Mo SteelAlloys and Steel UNS Table C Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 88 4 4 8.2 ASTM/ASME 8.2 A/SA-351 ASTM/ASME A/SA-358 CK3MCuN J93254 — S32053 93/43 [640/295] 888 4 4 8.1 4 ASTM/ASME8 8.1 A/SA-312 ASTM/ASME 8.3 A/SA-312 ASTM/ASME 4 S31725 A/SA-312 S31726 S31725 8.2 S34565 ASTM/ASME S31726 A/SA-358 S34565 S31254 S31254 75/30 [ 80/35 [550/ 115/60 [795/415] 94/45 88 4 4 8.2 ASTM/ASME 8.2 A/SA-312 ASTM/ASME A/SA-312 S31254 S31254 S31254 S31254 [>5] >0.1875 95/ 888 48 4 8.2 4 ASTM/ASME 8.1 4 A/SA-249 ASTM/ASME 8.1 A/SA-249 ASTM/ASME 8.2 S31254 A/SA-249 ASTM/ASME S31725 A/SA-312 S31254 S31726 S31725 [> >0.1875 S31726 — S32053 75/ 80/35 93/43 [640/295] Se 88 4 4 8.2 ASTM/ASME 8.2 A/SA-249 ASTM/ASME A/SA-249 — S31254 S31254 S32053 93/43 [640/295] Tube Welded 23Cr-25Ni-5.5Mo-N 8 4 8.3 ASTM/ASME A/SA-240 S34565 S34565 115/60 [795/415] 8 4 8.1 ASTM/ASME A/SA-240 S31726 S31726 80/35 [550/ 8 3 8.3 ASTM/ASME A/SA-814 TPXM-29 S24000 100/55 [690/ 888 38 38 8.3 4 ASTM/ASME8 8.3 4 A/SA-965 ASTM/ASME8 8.2 4 A/SA-965 ASTM/ASME8 8.2 FXM-11 4 A/SA-182 ASTM/ASME8 8.3 FXM-19 4 A/SA-182 S21904 ASTM/ASME 8.3 4 A/SA-182 S20910 ASTM/ASME — 8.1 4 A/SA-213 F44 ASTM/ASME 8.1 A/SA-213 F49 ASTM/ASME 8.2 S34565 S32053 A/SA-213 ASTM/ASME TP317LM S31254 A/SA-240 TP317LMN S34565 S34565 S31725 S31726 90/50 [620/345] — 100/55 [690/380] S32053 93/43 [640/295] Forgings 94/44 [650/305] Forgings 115/60 [795/ 115/60 [795/415] 75/ 80/ Forgings Forgings 21Cr-6Ni-9Mn 22Cr-13Ni-5Mn Forgings 93/43 [640/295] 23Cr-25Ni-5.5Mo-N 24Cr-17Ni-6Mn-4.5Mo-N Pl 20Cr-18Ni-6Mo 888 4 4 8.2 4 ASTM/ASME 8.2 A/SA-240 ASTM/ASME 8.1 A/SA-240 ASTM/ASME S31254 A/SA-240 S31254 S3125 S31725 S31254 S31725 100/45 75/30 [515/ Material Number
152 AWS B2.1/B2.1M-BMG:2014 Nominal Composition ttings 20Cr-18Ni-6Mo pe 19Cr-15.5Ni-4Mo Pipe 19Cr-15Ni-4Mo Worked Welded Pipe Welded Worked 23Cr-25Ni-5.5Mo-N Wrought Piping Fittings 23Cr-25Ni-5.5Mo-N 5] Wrought Piping Fittings 24Cr-17Ni-6Mn-4.5Mo-N 415] Seamless Pipe 24Cr-17Ni-6Mn-4.5Mo-N 305] Pipe Welded Worked Cold 20Cr-18Ni-6Mo 550/240] Pipe Fusion Welded 650/305] 19Cr-15.5Ni-4Mo Wrought Piping Fi 450/240]435/315]Pipe Seamless & Welded Pipe Seamless & Welded 2.5Ni 2Ni-1Cu [515/205] Pipe Fusion Welded [550/240] 19Cr-15Ni-4Mo Seamless Pi [550/240] Pipe Welded [550/240] 19Cr-15.5Ni-4Mo Bars & Shapes 19Cr-15.5Ni-4Mo 30 [515/205] Seamless 44 [650/305]30 [515/205] Pipe Welded Pipe Welded 44 [655/305]30 [515/205] 20Cr-18Ni-6Mo 19Cr-15Ni-4Mo Bars & Shapes Bars & Shapes44 [650/305] 20Cr-18Ni-6Mo 19Cr-15Ni-4Mo Pipe Welded 20Cr-18Ni-6Mo Minimum Minimum Tensile/Yield 63/46 [435/315] Piping Fittings 2Ni-1Cu Strength, ksi [MPa] Product Form in [mm] in Thickness or Diameter or Diameter Limitations, .2 (Continued) (Continued) SteelAlloys and Steel UNS Table C K21703K22103 65/37 [450/255] 70/40 [485/275] Plate Plate 2.5Ni 2.5Ni Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 8 4 8.1 ASTM/ASME A/SA-358 S31725 S31725 75/30 888 48 48 8.1 4 ASTM/ASME 8.1 4 A/SA-358 ASTM/ASME 8.1 4 A/SA-376 ASTM/ASME 8.3 S31726 A/SA-376 ASTM/ASME 8.2 S31725 A/SA-376 ASTM/ASME S31726 S31726 A/SA-403 S31725 S34565 S31726 S34565 — S31254 80/35 [ 75/ 80/35 115/60 [795/ 94/44 [ 888 48 48 8.2 4 ASTM/ASME8 8.3 4 A/SA-403 ASTM/ASME8 8.2 4 A/SA-403 ASTM/ASME8 8.2 4 A/SA-409 ASTM/ASME8 — 8.1 4 S34565 A/SA-409 ASTM/ASME8 8.1 4 A/SA-409 ASTM/ASME S345658 8.3 — 4 S31254 S32053 A/SA-409 ASTM/ASME8 8.2 4 S31725 A/SA-409 ASTM/ASME S312548 8.2 4 S31726 S32053 A/SA-479 ASTM/ASME S317258 8.1 4 S34565 A/SA-479 ASTM/ASME S317268 8.1 4 A/SA-479 ASTM/ASME S345658 — 8.3 4 S31254 A/SA-479 ASTM/ASME8 8.2 4 S31725 115/60 [795/41 A/SA-479 S31254 8.2 93/43 [640/295] 4 S31726 S32053 ASTM/ASME S31725 ASTM 8.2 4 S34565 A/SA-813 94/ ASTM/ASME S31726 8.2 93/43 [640/295] A/SA-813 75/ ASTM/ASME S34565 8.2 A743 A/SA-814 80/35 ASTM/ASME — S31254 115/60 [795/415] A/SA-814 CK3MCuN Pipe Welded S31254 — J93254 S31254 S32053 95/ 93/43 [640/295] 75/ Pipe Welded S31254 S32053 23Cr-25Ni-5.5Mo-N 80/35 115/60 [795/415] Bars & Shapes 24Cr-17Ni-6Mn-4.5Mo-N Bars & Shapes 94/ 80/38 [550/260] 93/43 [640/295] 23Cr-25Ni-5.5Mo-N 94/44 [650/ 24Cr-17Ni-6Mn-4.5Mo-N 93/43 [640/295] Pipe Welded Cold Castings 23Cr-25Ni-5.5Mo-N 20Cr-18Ni-6Mo 9A9A 19A 19A 9.1 19A ASTM/ASME 9.1 19A A/SA-182 ASTM/ASME 9.1 1 A/SA-203 ASTM/ASME 9.1 1 A/SA-203 ASTM/ASME FR 9.1 A/SA-234 ASTM/ASME 9.1 A A/SA-333 ASTM/ASME B K22035 A/SA-333 WPR 7 K22035 9 K21903 K22035 63/46 [435/315] Forgings 65/35 [ 63/46 [ 2Ni-1Cu Material Number
153 AWS B2.1/B2.1M-BMG:2014 Nominal Composition ng Fittings 3.5Ni 450/240]Pipe Seamless & Welded 3.5Ni Minimum Minimum Tensile/Yield 65/35 [450/240] Pipi 63/46 [435/315] Piping Fittings 2Ni-1Cu Strength, ksi [MPa] Product Form 51] 80/55 [550/380] Plate 3.5Ni ≤ 2 [ 2 [>51] 75/50 [515/345] Plate 3.5Ni in [mm] in ≤ Thickness or Diameter or Diameter Limitations, .2 (Continued) SteelAlloys and Steel UNS 31550 70/40 [485/275] Castings 3.5Ni 41500 70/40 [485/275] Castings 4.5Ni 22500 70/40 [485/275] Castings 2.5Ni Table C K31718K32018 65/37 [450/255] 70/40 [485/275] Plate Plate 3.5Ni 3.5Ni Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Specification M-Number Listing of Base Metals—Ferrous Alloys (see C.1, I2.2.1, and I3) I2.2.1, C.1, (see Alloys Metals—Ferrous of Base M-Number Listing ISO 15608 15608 Group Standard Group Group Number 9B9B 1 1 9.2 ASTM/ASME 9.2 A/SA-203 ASTM/ASME A/SA-203 E F — > 9B 1 9.2 ASTM/ASME A/SA-203 D 9B9B 19B 19B 9.2 19B ASTM/ASME 9.2 19B A/SA-203 ASTM/ASME 9.2 1 A/SA-333 ASTM/ASME 9.2 1 A/SA-334 ASTM/ASME 9.3 F A/SA-350 ASTM/ASME 9.2 3 A/SA-352 ASTM/ASME 3 A/SA-420 LF3 — K31918 LC3 WPL3 K31918 K32025 J K31918 65/35 [ [485/260] 70/37.5 65/35 [450/240] Tube Welded Forgings 3.5Ni 3.5Ni 9B9B 19B 19B — 19B — 19B — ASTM 19B — ASTM 19C — ASTM 1 A707 — ASTM 1 A707 9.2 ASTM A707 L7, Cl. 1 ASTM/ASME 9.3 ASTM A707 A/SA-765 L7, Cl. 2 ASTM/ASME K32218 A707 A/SA-352 L8, Cl. 1 K32218 A707 L8, Cl. 2 III K42247 L8, Cl. 3 LC4 K42247 L8, Cl. 4 K42247 K32026 J K42247 60/42 [415/290] 66/52 [455/360] 60/42 [415/290] 66/52 [455/360] [485/260] 70/37.5 75/60 [515/415] Forgings 90/75 [620/515] Forgings Forgings Forgings Forgings Forgings Forgings 3.5Ni-1.8Cr-0.5Mo-0.3Mn 3.5Ni 3.5Ni-1.8Cr-0.5Mo-0.3Mn 3.5Ni 3.5Ni-1.8Cr-0.5Mo-0.3Mn 3.5Ni-1.8Cr-0.5Mo-0.3Mn 3.5Ni 9A9A 19A 1 9.1 1 ASTM/ASME 9.1 A/SA-420 9.1 ASTM WPL9 ASTM K22035 A714 A714 V E V, K22035 K22035[450/315] 65/46 65/46 [450/315]Pipe Seamless & Welded Pipe Seamless & Welded 2Ni-1Cu 2Ni-1Cu 9A9A 19A 19A 9.1 19A ASTM/ASME 9.1 19A A/SA-334 ASTM/ASME 9.1 1 A/SA-334 ASTM/ASME 9.1 1 A/SA-350 ASTM/ASME 9.1 7 A/SA-350 ASTM/ASME LF5, 1Cl. 9.1 9 A/SA-350 ASTM/ASME LF5, 2Cl. K13050 A/SA-352 K21903 K13050 K22035 LF9 LC2 K22036 J 60/30 [415/205] 65/35 [450/240] [485/260] 70/37.5 63/46 [435/315] 63/46 [435/315] Tube Welded Forgings Forgings Tube Welded Forgings 2.5Ni 2Ni-1Cu 1.5Ni 1.5Ni 2Ni-1Cu Material Number
154 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition [76/21]Rod, & Wire Bar, 99.0Al-Cu [55/17] & Sheet Plate 99.60Al 5 [97/34]5 Plate & Sheet Al-Mn-Cu 6 [125/41]6 Plate & Sheet Al-1.5Mg 4.5 [90/31] Seamless Tube Al-Mn-Cu 4.5 [90/31]Shapes& Rod, Bar, Al-Mn-Cu Minimum 3/4.5 [90/31] Seamless Tube Al-Mn-Cu 14/5 [97/34] 14/5 Plate & Sheet Al-Mn-Cu Tensile/Yield 13/4.5 [90/31] Plate & Sheet Al-Mn-Cu Strength, ksi [MPa] Produc 3 76] ≤ .2 ≤ 13][97/34] 14/5 Plate & Sheet Al-Mn-Cu inum Base Alloys ≥ [<13] [90/31] 13/4.5 Plate & Sheet Al-Mn-Cu 0.5 [ in [mm] in 0.5 and 0.5 and Diameter 13 and 13 ≥ ≥ Limitations, ≥ Thickness or [ (Continued) [>1.3 and <13] and [>1.3 Table C UNS Number Aluminum and Alum or Alloy Type, Grade, Type, Specification Base Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 Group Standard 2121 2121 2121 ASTM/ASME 22.121 ASTM/ASME B/SB-209 22.2 ASTM/ASME B/SB-209 ASTM/ASME — B/SB-209 1060 B/SB-209 ASTM/ASME21 1100 3003 B/SB-209 A91060 5050 — Alclad 3003 A91100 A93003 ASTM/ASME A95050 — B/SB-209 Alclad 3003 A83003 8/2.5 [76/24] 11/3.5 14/ 18/ Plate & Sheet 99.0Al-Cu 21 —21 ASTM/ASME21 B/SB-209 —21 2121 Alclad 3003 ASTM/ASME 2121 ASTM/ASME B/SB-209 22.121 — B/SB-210 22.1 ASTM/ASME Alclad 300321 ASTM — B/SB-21021 A83003 >0.05 and <0.5 22.2 ASTM 106021 —21 B210 <0.5 ASTM 3003 ASTM —21 A91060 ASTM/ASME B210 —21 B/SB-210 A93003 —21 B210 1100 ASTM B210 Alclad 3003 2121 ASTM 3102 2121 ASTM/ASME ASTM A91100 22.1 —21 B210 ASTM/ASME 3303 B/SB-211 ASTM/ASME 5050 2121 A93102 B210 B/SB-211 21 B/SB-21121 B210 8.5/2.5 [59/17] ASTM/ASME 3003 Alclad A93303 22.1 106021 A95050 ASTM/ASME 3102 Alclad B/SB-221 A83003 22.1 ASTM/ASME 110021 [97/34] 14/5 3303 Alclad 3003 B/SB-221 ASTM/ASME Seamless Tube — B/SB-221 A91060 — 1060 21 B/SB-221 A91100 ASTM/ASME — [76/24] 11/3.5 A93003 1100 Seamless Tube 3003 B/SB-221 1 A91060 ASTM 3102 [82/28] 12/4 Alclad 3003 A91100 Seamless Tube A93003 99.60Al [97/34] 14/5 A83003 18/6 [125/41] 13/ A93102 B230 Seamless Tube Al-Mn-Cu 8/2.5 [55/17] Seamless Tube Seamless Tube [69/24] 10/3.5 11/3 [97/34] 14/5 99.0Al-Cu [90/31] 13/4.5 1350 Rod, & Wire Bar, 8.5/2.5 [59/17] Seamless Tube Al-0.3Mg [76/21] 11/3 Rod, & Wire A91350 Bar, Seamless Tube [97/34] 14/5 & ShapesRod, Bar, 13/ Al-1.5Mg [82/28] 12/4 Al-Mn & ShapesRod, Bar, & ShapesRod, Bar, 99.60Al & ShapesRod, Bar, Al-0.3Mg Al-Mn-Cu 99.60Al Al-Mn 99.0Al-Cu Al-Mn-Cu [55/–] 8/– Al-0.3Mg Wire 99.50Al Material Number
155 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition [59/17] Seamless Pipe & Tube 99.60Al [90/31] Seamless Pipe & Tube Al-Mn-Cu 76/21] Seamless Pipe & Tube 99.0Al-Cu [97/34] Seamless Pipe & Tube Al-Mn-Cu 5 [90/31]Tube& Seamless Pipe Al-Mn-Cu 4.5 [90/31]Tube& Seamless Pipe Al-Mn-Cu 1/4 [76/28]1/4 Forgings 99.0Al-Cu Minimum 3/4.5 [90/31] Seamless Tube Al-Mn-Cu Tensile/Yield Strength, ksi [MPa] Produc inum Base Alloys in [mm] in Diameter Limitations, .2 (Continued) Thickness or (Continued) 3 [90/31] 13/4.5 Seamless Tube Al-Mn-Cu Table C UNS Number Aluminum and Alum or Alloy Type, Grade, Type, Specification Base Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 Group Standard 2121 —21 2121 ASTM/ASME 2121 B/SB-234 2121 ASTM/ASME ASTM 22.1 Alclad 300321 ASTM/ASME B/SB-241 ASTM/ASME —21 A8300 B/SB-241 — B/SB-24121 B236 ASTM/ASME 1060 2121 ASTM/ASME B/SB-241 22.1 110021 ASTM/ASME 3003 B/SB-241 ASTM/ASME Alclad 3003 2121 A91060 1350 B/SB-247 22.1 Alclad 3003 B/SB-24721 A91100 22.2 A93003 —21 A83003 ASTM A91350 ASTM 1100 2121 3003 ASTM 2121 22.121 B313 A91100 ASTM B313 A93003 —21 ASTM B313 ASTM —21 8.5/2.5 2121 B324 1100 ASTM [ 11/3 3003 2121 14/5 B345 13/ ASTM 22.1 B345 5050 13/4. 21 [55/–] 8/– ASTM A91100 2121 A93003 B345 1350 ASTM ASTM 2121 A95050 B361 1060 1 3003 2121 [97/34] 14/5 B361 3003 Alclad ASTM A91350 Alclad 3003 WP 22.121 B361 ASTM A83003 A83003 A91060 22.1 B361 A93003 Bar ASTM 22.2 WP1060 ASTM B483 WP1100 ASTM Forgings B483 WP3003 A91060 [76/24] 11/3.5 ASTM B483 [97/34] 14/5 A91100 B483 A93003 18/6 [125/41] 1060 B483 1100 Tube Welded B483 8.5/– [59/–] 1435 [90/31] 13/4.5 Tube 8.5/2.5 [59/17] Welded A91060 13/4.5 3003 99.50Al Tube Welded Al-Mn-Cu [97/34] 14/5 A91100 3102 Seamless Pipe & Tube A91435 5050 A93003 Seamless Pipe & Tube 8.5/2.5 [59/17] A93102 Fittings Wire 99.0Al-Cu [76/21] 11/3 A95050 [97/34] 14/5 Al-Mn-Cu 99.60Al Al-1.5Mg Al-Mn-Cu Fittings 8.5/2.5 [59/17] [76/24] 11/3.5 Fittings Fittings 9.5/3 [66/21] Al-Mn-Cu [97/34] 14/5 99.50Al [76/24] 11/3.5 Tube 18/6 [125/41] Tube 99.60Al Tube 99.0Al-Cu Tube Al-Mn-Cu Tube Tube 99.60Al 99.0Al-Cu 99.35Al-Fe Al-Mn-Cu Al-0.3Mg Al-1.5Mg 2121 2121 22.1 ASTM/ASME ASTM/ASME — B/SB-234 B/SB-234 ASTM/ASME B/SB-234 1060 3003 Alclad 3003 A91060 A93003 — 8.5/2.5 [59/17] [97/34] 14/5 1 Seamless Tube Seamless Tube 99.60Al Al-Mn-Cu Material Number
156 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition & Sheet Al-Mn-Mg [215/83][110/–] & Sheet Plate Plate & Sheet Al-2.7Mg-Mn Al-1Mg-0.3Mn [105/34] Plate & Sheet Al-0.4Mg-0.2Mn 5 [97/34]5 Plate & Sheet Al-Mn-Mg 5 [105/34]5 Plate & Sheet Al-1.5Mg 8.5 [150/59]8.5 [115/45]6.5 Plate & Sheet Plate & Sheet[170/66]9.5 [170/66]9.5 Al-Mn-Mg Plate & Sheet Al-Mn-Mg Plate & Sheet[170/66]9.5 Al-2.5Mg Plate & Sheet Al-2.5Mg Al-2.5Mg Minimum Tensile/Yield 21/8 [145/55]21/8 Plate & Sheet Al-Mn-Mg 22/8.5 [150/59] Plate Strength, ksi [MPa] Produc 3 76] ≤ ≤ 13][150/59] 22/8.5 Plate & Sheet Al-Mn-Mg inum Base Alloys ≥ [<13][145/55] 21/8 Plate & Sheet Al-Mn-Mg 0.5 [ in [mm] in 0.5 and 0.5 and Diameter 13 and 13 ≥ ≥ Limitations, .2 (Continued) ≥ Thickness or [ (Continued) [>1.3 and <13] and [>1.3 Table C UNS Number Aluminum and Alum or Alloy Type, Grade, Type, Specification Base Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 Group Standard 2222 22.222 22.2 ASTM/ASME22 22.2 ASTM/ASME B/SB-20922 22.2 ASTM/ASME B/SB-20922 22.3 ASTM/ASME B/SB-20922 3005 22.4 ASTM/ASME B/SB-20922 3105 22.3 ASTM/ASME B/SB-20922 5005 22.4 A93005 ASTM/ASME B/SB-20922 5010 22.3 A93105 ASTM/ASME B/SB-20922 5052 22.2 A95005 ASTM/ASME B/SB-20922 5154 22.3 A95010 ASTM/ASME B/SB-209 5252 A95052 ASTM/ASME — B/SB-209 5254 A95154 B/SB-209 ASTM/ASME 5454 A95252 5457 B/SB-209 17/ A95254 5652 A95454 Alclad 3004 14/ A95457 15/ A95652 15/5 — 25/ [205/76] 30/11 25/ [205/76] 30/11 & Sheet Plate 31/12 16/– & Sheet Plate 25/ Al-3.5Mg Al-3.5Mg 2121 2121 2121 2121 ASTM 2121 ASTM 22.121 ASTM 22.121 B491 ASTM ASTM 2121 B491 22.1 ASTM21 B491 22.221 B491 1050 ASTM B491 ASTM —22 1100 B491 ASTM 21 1200 A91050 22.2 B547 1235 ASTM A91100 B547 ASTM/ASME 3003 ASTM A91200 B547 3102 B/SB-209 A91235 A93003 B547 1100 3003 A93102 B609 3004 5050 3003 Alclad A91100 A93003 A83003 A93004 8/2.5 [55/17] A95050 1350 [76/21] 11/3 [76/66] 11/9.5 A91350 Tube Extruded 9/3 [62/21] [97/34] 14/5 Extruded Tube [76/24] 11/3.5 Tube Extruded [76/24] 11/3.5 Extruded Tube Extruded Tube [97/34] 14/5 22/ [90/31] 13/4.5 Tube Extruded 18/6 [125/41] 99.5Al-Fe Tube Welded 99.0Al-Cu 99.0Al-Si-Fe Tube Tube Welded Welded 8.5/– [59/–] Tube Welded 99.5Al-Fe Al-Mn-Cu Al-0.3Mg 99.0Al-Cu Wire Al-Mn-Cu Al-Mn-Cu Al-1.5Mg 99.50Al 2222 — — ASTM/ASME ASTM/ASME B/SB-209 B/SB-209 Alclad 3004 Alclad 3004 — — <0.5 >0.05 and <0.5 22 — ASTM/ASME B/SB-209 Alclad 3004 — Material Number
157 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition 83] Seamless Pipe & Tube Al-2.7Mg-Mn 170/69] Seamless Pipe & Tube Al-2.5Mg [160/59] & ShapesRod, Bar, Al-Mn-Mg [215/83] Tube Seamless Al-2.7Mg-Mn 5 [170/66] Rod, & Wire Bar, Al-2.5Mg – [165/–]– Plate & Sheet Al-Mg-Si-Cu 10 [170/69]11 [205/76] Seamless Tube Seamless Tube Al-2.5Mg 10 [170/69] Al-3.5Mg Seamless Tube Al-2.5Mg 4/– [165/–] 4/– Plate & Sheet Al-Mg-Si-Cu Minimum Tensile/Yield Strength, ksi [MPa] Produc inum Base Alloys in [mm] in Diameter Limitations, .2 (Continued) Thickness or (Continued) Table C UNS Number Aluminum and Alum or Alloy Type, Grade, Type, Specification Base Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 Group Standard 2222 22.2 22.3 ASTM/ASME ASTM B/SB-210 B210 5052 A95052 5005 A95005 25/ 15/5 [105/34] Seamless Tube Al-1.5Mg 2222 22.422 22.3 ASTM/ASME22 22.4 ASTM/ASME B/SB-21022 22.2 ASTM/ASME B/SB-21122 22.3 ASTM/ASME B/SB-21122 5154 22.4 ASTM/ASME B/SB-22122 5052 22.3 ASTM/ASME B/SB-22122 5154 22.3 A95154 ASTM/ASME B/SB-22122 3004 22.3 A95052 ASTM/ASME B/SB-22122 5052 22.3 A95154 ASTM/ASME B/SB-23422 5154 22.3 A93004 ASTM/ASME B/SB-23422 5454 22.2 A95052 ASTM/ASME B/SB-24122 5052 22.2 A95154 B/SB-24122 5454 22.3 A95454 ASTM22 5052 22.4 30/ A95052 ASTM22 5454 25/9. A95454 ASTM —22 22.3 B313 30/11 [205/76] A95052 ASTM22 23/8.5 22.2 B313 A9545422 ASTM 22.2 B313 25/10 [170/69] ASTM Rod, & Wire Bar, 22 22.3 B313 30/11 [205/76] 3004 ASTM22 & ShapesRod, Bar, 22.2 31/12 [215/83] 3005 ASTM22 B313 & ShapesRod, Bar, 22.3 B361 25/ 5052 ASTM22 A93004 & ShapesRod, Bar, 22.4 B396 31/12 5154 ASTM22 A93005 3004 Alclad Al-3.5Mg 22.3 B483 25/10 [ ASTM23 A95052 B483 31/12 [215/ Al-2.5Mg 5154 ASTM —23 A95154 — 23.1 B547 Al-3.5Mg 5005 ASTM Al-2.7Mg-Mn B547 ASTM/ASME 5005 — A95154 ASTM B547 5052 B/SB-209 A95005 ASTM/ASME B547 3004 22/8.5 [150/59] A95005 B/SB-209 5052 17/6.5 [115/45] A95052 B547 6061 5154 Alclad 6061 25/9.5 [170/66] A93004 Tube 5454 Welded 30/11 [205/76] A95052 3004 Alclad Tube A96061 Welded — A95154[145/55] 21/8 Tube Welded 30/11 [205/76] A95454 — Tube Welded 15/5 [105/34] 15/5 [105/34] Tube Welded Al-Mn-Mg 25/9.5 [170/66] Al-Mn-Mg Fittings 22/8.5 [150/59] Al-2.5Mg 25/9.5 [170/66] Wire Al-3.5Mg 24/ 30/11 [205/76] Tube Tube Welded Tube 31/12 [215/83] 2 Al-Mn-Mg Tube Welded [145/55] 21/8 Tube Welded Al-3.5Mg Tube Welded Tube Welded Al-Mn-Mg Al-1.5Mg Al-1.5Mg Al-2.5Mg Al-2.5Mg Al-3.5Mg Al-2.7Mg-Mn Al-Mn-Mg Material Number
158 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition 165/–] Seamless Pipe & Tube165/–] Seamless Pipe & Tube Al-Mg-Si-Cu Al-Si-Mg-Mn [115/–][165/–] Seamless Pipe & Tube Seamless Pipe & Tube Al-Mg-Si Al-Si-Mg Minimum Tensile/Yield Strength, ksi [MPa] Produc 13][165/–] 24/– Plate & Sheet Al-Mg-Si-Cu inum Base Alloys ≥ [<13][160/–] 23/– Plate & Sheet Al-Mg-Si-Cu 0.5 [ in [mm] in Diameter ≥ Limitations, .2 (Continued) Thickness or (Continued) Table C UNS Number Aluminum and Alum or Alloy Type, Grade, Type, Specification Base Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 Group Standard 23 — ASTM/ASME B/SB-209 Alclad 6061 A86061 23 — ASTM/ASME B/SB-209 Alclad 6061 A86061 <0.5 2323 23.123 23.1 ASTM/ASME23 23.1 ASTM/ASME B/SB-21023 23.1 ASTM/ASME B/SB-21023 23.1 ASTM/ASME B/SB-21123 6061 23.1 ASTM/ASME B/SB-22123 6063 23.1 ASTM/ASME B/SB-22123 6061 23.1 A96061 ASTM/ASME B/SB-22123 6005 23.1 A96063 ASTM/ASME B/SB-22123 6005A 23.1 A96061 ASTM/ASME B/SB-22123 6061 23.1 A96005 ASTM/ASME B/SB-22123 A96005 6063 23.1 ASTM/ASME B/SB-22123 6105 23.1 A96061 ASTM/ASME B/SB-22123 6162 23.1 A96063 ASTM/ASME B/SB-23423 6351 23.1 A96105 ASTM/ASME B/SB-24123 [165/–] 24/– 6463 23.1 A96162 ASTM/ASME B/SB-24123 [115/–] 17/– 6061 23.1 A96351 ASTM/ASME B/SB-24123 [165/–] 24/– 6061 23.1 A96463 ASTM/ASME B/SB-241 Seamless Tube23 [165/–] 24/– 6063 [165/–] 24/– 23.1 A96061 ASTM/ASME B/SB-247 Seamless Tube23 6162 Rod, & Wire Bar, 23.1 A96061 ASTM/ASME B/SB-24723 [165/–] 24/– & ShapesRod, Bar, 6351 23.1 A96063 & ShapesRod, Bar, B/SB-30823 [115/–] 17/– 6061 23.1 A96162 ASTM23 [165/–] 24/– Al-Mg-Si-Cu & ShapesRod, Bar, 6151 23.1 A96351 ASTM23 [165/–] 24/– & ShapesRod, Bar, 6061 Al-Mg-Si-Cu 23.1 A96061 ASTM Al-Mg-Si 23 [165/–] 24/– & ShapesRod, Bar, Al-Si-Mg 23.1 B313 A96151 ASTM Al-Si-Mg 23 [115/–] 17/– & ShapesRod, Bar, 23.1 B317 A96061 ASTM Al-Mg-Si-Cu [165/–] 24/– & ShapesRod, Bar, 23.1 B345 ASTM [ 24/– & ShapesRod, Bar, Al-Mg-Si B345 6061 ASTM 17/– Al-Si-Mg B345 6101 ASTM Seamless Tube 24/– Al-Si-Mg B361 6061 Al-Si-Mg-Mn [ 24/– A96061 B361 6063 [165/–] 24/– A96101 Al-Si-Mg B429 6351 [165/–] 24/– A96061 WP6061 [165/–] 24/– A96063 WP6063 Al-Mg-Si-Cu A96061 A96351 6061 Forgings A96063 Forgings Shapes A96061 [165/–] 24/– [76/–] 11/– [165/–] 24/– Al-Mg-Si-Cu Shapes, & Tube Rod, Bar, [115/–] 17/– Tube Welded Al-Mg-Si-Cr Seamless Pipe & Tube [165/–] 24/– [165/–] 24/– Seamless Pipe & Tube [115/–] 17/– Al-Mg-Si-Cu Seamless Pipe & Tube Al-Mg-Si [165/–] 24/– Al-Mg-Si-Cu Al-Mg-Si-Cu Fittings Al-Mg-Si Fittings Al-Si-Mg-Mn Pipe & Tube Al-Mg-Si-Cu Al-Mg-Si Al-Mg-Si-Cu Material Number
159 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition less Pipe & Tube Al-4.5Cu-1Si-0.8Mn-0.6Mg Plate & Sheet Al-4.5Cu-1Si-0.8Mn-0.6Mg Bar, Rod, & Wire Bar, Al-6Cu-0.3Mn-Ti-Zr Seamless Pipe & Tube Al-6Cu-0.3Mn-Ti-Zr 240/–] Plate & Sheet Al-4.5Cu-1Si-0.8Mn-0.6Mg [240/97] & Sheet Plate Al-4.0Mg-Mn [240/–] Forgings Al-6Cu-0.3Mn-Ti-Zr – [240/–]– Plate & Sheet Al-6Cu-0.3Mn-Ti-Zr Minimum Tensile/Yield 36/14 [250/97]36/14 & Sheet Plate Al-4.4Mg-Mn 39/17 [270/115]39/17 Plate & Sheet Al-4.4Mg-Mn 40/18 [275/125]40/18 Plate & Sheet[255/105]37/15 Plate & Sheet Al-4.4Mg-Mn [260/110]38/16 Plate & Sheet Al-4.4Mg-Mn Al-4.4Mg-Mn Strength, ksi [MPa] Produc 3 1.5 38] 76] 5 8 203] 7 178] ≤ 127] ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ inum Base Alloys in [mm] in Diameter Limitations, .2 (Continued) Thickness or [>38 and [>38 and (Continued) [>1.3 and [>76 and [>178 and [>178 and [>127 and Table C UNS Number Aluminum and Alum or Alloy Type, Grade, Type, Specification Base Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 Group Standard 25 22.4 ASTM/ASME B/SB-209 5083 A95083 >3 and 25 22.425 ASTM/ASME 22.425 B/SB-209 ASTM/ASME 22.4 B/SB-209 ASTM/ASME 508325 B/SB-209 5083 A95083 22.4 ASTM/ASME 5083 A95083 >7 and B/SB-209 A95083 >5 and 5086 and >1.5 A95086 35/14 2424 2625 26 ASTM/ASME 22.4 ASTM/ASME B/SB-247 ASTM/ASME B/SB-247 B/SB-209 2014 2219 5083 A92014 A92219 A95083 >0.05 and [240/–] 35/– 35/– Forgings Al-4.5Cu-1Si-0.8Mn-0.6Mg 2424 2624 2624 ASTM/ASME 26 ASTM/ASME B/SB-221 26 ASTM/ASME B/SB-221 ASTM/ASME B/SB-241 2014 B/SB-241 2219 2014 A92014 2219 A92219 A92014 A92219 [240/–] 35/– [240/–] 35/– [240/–] 35/– & ShapesRod, Bar, [240/–] 35/– & ShapesRod, Bar, Al-4.5Cu-1Si-0.8Mn-0.6Mg Seam Al-6Cu-0.3Mn-Ti-Zr 2424 2624 —24 ASTM/ASME —24 ASTM/ASME B/SB-209 2624 ASTM/ASME B/SB-209 26 B/SB-209 Alclad 2014 2219 26 ASTM/ASME ASTM Alclad 2219 A82014 ASTM/ASME B/SB-211 A82219 A92219 B/SB-211 B210 2014 2219 A92014 2014 A92219[ 35/– A92014 35/ [240/–] 35/– Plate & Sheet [240/–] 35/– [240/–] 35/– [240/–] 35/– Al-6Cu-0.3Mn-Ti-Zr Rod, & Wire Bar, Al-4.5Cu-1Si-0.8Mn-0.6Mg Seamless Tube Al-4.5Cu-1Si-0.8Mn-0.6Mg 2323 23.123 23.123 23.1 ASTM23 23.1 ASTM23 23.1 ASTM24 23.1 B429 ASTM B483 ASTM 26 B483 ISO ASTM/ASME B491 6063 B/SB-209 B547 6061 6063 A96063 209 6063 2014 A96061 6061 A96063T4, T6 6082, A96063 A92014 A96061 A96082 [115/–] 17/– [165/–] 24/– [115/–] 17/– [115/–] 17/– [240/–] 35/– Pipe & Tube [165/–] 24/– [165/–] 24/– TubeShapes, & Tube Rod, Bar, Extruded Tube Tube Tube Welded Al-1Si-Mg-Mn Al-Mg-Si Al-Mg-Si Al-Mg-Si-Cu Al-Mg-Si-Cu Al-Mg-Si Material Number
160 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition 97] Seamless Pipe & Tube Al-4.0Mg-Mn 270/110] Seamless Pipe & Tube285/130] Seamless Pipe & Tube Al-4.4Mg-Mn Al-5.1Mg-Mn [255/–]Rod, & Wire Bar, Al-5Mg-Mn-Cr Minimum Tensile/Yield 39/16 [270/110]39/16 [260/105]38/15 Plate & Sheet[290/130]42/19 Plate & Sheet Plate & Sheet Al-5.1Mg-Mn Al-5.1Mg-Mn Al-5.1Mg-Mn 39/16 [270/110]39/16 Plate & Sheet Al-4.4Mg-Mn 41/18 [285/125]41/18 Plate & Sheet Al-5.1Mg-Mn 40/17 [275/115]40/17 Plate & Sheet Al-5.1Mg-Mn Strength, ksi [MPa] Produc 3 3 1.5 38] 7 178] 8 203] 5 76] 76] ≤ ≤ ≤ 127] ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ inum Base Alloys in [mm] in Diameter Limitations, .2 (Continued) Thickness or [>38 and [>38 and [>38 and [>38 and (Continued) >76 and [>1.3 and [>127 and [>127 and [>178 and Table C UNS Number Aluminum and Alum or Alloy Type, Grade, Type, Specification Base Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 Group Standard 25 22.4 ASTM/ASME B/SB-209 5456 A95456 >5 and 25 22.425 ASTM/ASME 22.425 B/SB-209 ASTM/ASME 22.4 B/SB-209 ASTM/ASME 5456 B/SB-209 5456 A95456 5456 A95456 >7 and >0.05 and A95456 >3 and 2525 22.425 22.425 22.4 ASTM25 22.4 ASTM25 ASTM/ASME ASTM —25 22.4 B210 B/SB-21125 ASTM/ASME 22.4 B210 ASTM/ASME25 B/SB-211 22.4 B210 ASTM/ASME B/SB-22125 5056 22.4 ASTM/ASME 5083 Alclad 5056 B/SB-22125 22.4 ASTM/ASME 5086 B/SB-22125 5083 22.4 A95056 ASTM/ASME 5456 B/SB-241 —25 A95083 5086 22.4 ASTM/ASME B/SB-24125 A95086 5456 22.4 A95083 ASTM/ASME B/SB-24125 A95456 5083 22.4 A95086 B/SB-24725 5086 22.4 A95456 ASTM25 5456 22.4 A95083 ASTM25 5083 22.4 A95086 ASTM25 22.4 B313 A95456 ASTM 39/16 [270/110] [260/–] 38/– 22.4 B345 A95083 ASTM 35/14 [240/97] 37/– 39/16 [270/110] B345 ASTM/ASME ASTM 41/19 [285/130] Seamless Tube Rod, & Wire Bar, B361 35/14 [240/97] 5086 B/SB-928 & ShapesRod, Bar, 41/19 [285/130] Seamless B547Tube 5083 Seamless Tube 39/16 [ & ShapesRod, Bar, B547 5086 A95086 & ShapesRod, Bar, 5083 35/14 [240/ 5083 A95083 Al-5Mg-Mn-Cr 41/19 [ Al-4.4Mg-Mn 5083 Al-4.4Mg-Mn A95086 38/16 [260/110] A95083 5086 Al-4.0Mg-Mn A95083 Al-4.0Mg-Mn Al-5.1Mg-Mn Al-5.1Mg-Mn A95083 and >1.5 A95086 Forgings 35/14 [240/97] 39/16 [270/110] 35/14 [240/97] Seamless Pipe & Tube Tube 39/16 [270/110] Welded Seamless Pipe & Tube Al-4.4Mg-Mn 40/18 [275/125] 35/14 [240/97] Al-4.4Mg-Mn Fittings Tube Welded Al-4.0Mg-Mn Al-4.0Mg-Mn Tube Welded Al-4.4Mg-Mn Al-4.4Mg-Mn Al-4.0Mg-Mn 25 22.4 ASTM/ASME B/SB-209 5456 A95456 and >1.5 Material Number
161 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition – [165/–]– [195/–] Castings Castings Al-5.5Si-4.5Cu Al-9Si-3.5Cu-Mg 14 [170/97] Castings Al-8Si-1Cu-Mn-Mg Minimum Tensile/Yield 22/9 [150/62] Castings Al-4Mg-Si 19/12 [130/83] Castings Al-3Si-4Cu 27/14 [185/97] Castings Al-6Si-3Cu 35/14 [240/97]35/14 & Sheet Plate Al-4.0Mg-Mn 41/19 [285/130]41/19 Plate & Sheet Al-5.1Mg-Mn 34/21 [235/145] Castings Al-8Si-1Cu-Mn-Mg 30/17 [205/115] Castings Al-3Zn-Mg-Mn-Cr Strength, ksi [MPa] Produc 2 3 51] ≤ 76] ≤ ≤ ≤ inum Base Alloys in [mm] in Diameter Limitations, .2 (Continued) Thickness or [>38 and [>38 and (Continued) [>1.3 and 00000 [160/–] 23/– 23/13 [160/90] 23/13 [160/90] 31/20 [215/140] Castings0 Castings Castings 19/9.5 [130/66] Castings Al-Cu-Mg Castings Al-6Si-3Cu Al-6Si-3Cu 17/7 [115/48] Al-6Si-3Cu 0 Castings Al-Si-Mg 17/6 [115/41] Al-Si Castings Al-Si Table C 03560035600356003560 23/16 [160/110] 30/20 [205/140]07100 [215/–] 31/– 25/18 [170/125]13560 Castings13560 Castings Castings Castings 32/20 [220/140] Al-Si-Mg 34/24 [235/165] Al-Si-Mg 35/26 [240/180] Al-Si-Mg Al-Si-Mg Castings Castings Castings Al-6Zn-Mg Al-Si-Mg Al-Si-Mg UNS Number Aluminum and Alum or Alloy Type, Grade, Type, Specification Base Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 Group Standard 2626 2526 —26 ASTM/ASME —26 ASTM/ASME B/SB-26 2526 ASTM/ASME B/SB-26 2526 ASTM/ASME B/SB-26 2526 208.0 ASTM/ASME B/SB-26 222.0, O 2526 ASTM/ASME 222.0, T61 B/SB-26 2526 ASTM/ASME A02080 A0222 B/SB-26 24.2 319.0, F A02220 ASTM/ASME T5 319.0, B/SB-26 24.2 ASTM/ASME T6 319.0, B/SB-26 A0319 ASTM/ASME B/SB-26 A0319 328.0, F B/SB-26 A0319 T6 328.0, 26 356.0, F A03280 356.0, T5126 A03280 23.126 A0356 A 23.1 ASTM/ASME26 [205/–] 30/– ASTM/ASME —26 B/SB-26 23.2 B/SB-26 ASTM/ASME 23.2 ASTM/ASME 512.0 B/SB-26 ASTM/ASME Castings B/SB-26 514.0 25/ 26 B/SB-26 A0512026 T5 705.0, 535.0 A05140 2526 T5 710.0, A07050 25 ASTM/ASME A05350 A 25 ASTM/ASME B/SB-108 Al-Cu-Mg ASTM/ASME B/SB-108 B/SB-108 308.0 319.0 17/10 [115/69] 333.0, F A03080 A03190 35/18 [240/125] A03330 Castings Castings 24/ Al-4Mg-2Si 28/ Al-7Mg-Mn 25 22.4 ASTM/ASME B/SB-928 5086 A95086 and >0.05 2626 24.226 24.2 ASTM/ASME26 24.2 ASTM/ASME B/SB-26 24.1 ASTM/ASME B/SB-26 ASTM/ASME T6 356.0, B/SB-26 T7 356.0, B/SB-26 A 356.0, T71 A 26 A 443.026 24.226 24.2 ASTM/ASME A0443 24.1 ASTM/ASME B/SB-26 ASTM/ASME B/SB-26 T6 A356.0, B/SB-26 T61 A356.0, A A B443.0 A2443 25 22.4 ASTM/ASME B/SB-928 5456 A95456 and >1.5 Material Number
162 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition [150/62] Castings Al-4Mg-Si 8/– [195/–]8/– [195/–]8/– [195/–]8/– Castings Castings Castings Al-9Si-3.5Cu-Mg Al-9Si-3.5Cu-Mg Al-9Si-3.5Cu-Mg Minimum Tensile/Yield Strength, ksi [MPa] Produc inum Base Alloys in [mm] in Diameter Limitations, .2 (Continued) Thickness or 0 28/26 [195/180] Castings Al-Si-Mg Table C UNS Number Aluminum and Alum or Alloy Type, Grade, Type, Specification Base Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 Group Standard 26 25 ASTM/ASME B/SB-108 T5 333.0, A03330 2 2626 2526 2526 ASTM/ASME 24.226 ASTM/ASME B/SB-108 24.2 ASTM/ASME26 B/SB-108 24.2 ASTM/ASME B/SB-10826 T6 333.0, 24.1 ASTM/ASME B/SB-10826 T7 333.0, 23.2 ASTM/ASME 356.0, F B/SB-108 A0333026 T6 356.0, ASTM/ASME — B/SB-108 A0333026 356.0, T71 24.2 A03560 B/SB-10826 ASTM/ASME A03560 24.1 ASTM/ASME26 A03560 443.0 B/SB-108 24.1 ASTM/ASME B/SB-10826 513.0 ASTM/ASME 25 B/SB-10826 A04430 535.0 25 B/SB-10826 A356.0 A05130 2526 A444.0 2 ASTM 24.226 A1356 B443.0 A05350 2 ASTM 24.1 21/10 [145/69]26 A14440[230/150] 33/22 ASTM 23.1 ASTM26 A24430 B618 [160/–] 23/– ASTM —26 B618 24.2 ASTM26 B618 Castings Castings 24.1 21/7 [145/48] B61827 208.0 ASTM 22/12 [150/83] 24.2 B618 ASTM27 319.0 Castings 23.2 B618 ASTM 35/18 [240/125] 328.0 A02080 356.0 23.2 ASTM/ASME ASTM B618 [115/–] Castings 17/– A03190 443.0 B618 B/SB-221 Castings 21/6 [145/41] A03280 514.0 B618 A03560 Al-Si-Mg Castings ISO Al-Si-Mg B686 A04430 535.0 7005 A356.0 A05140 Al-Si-Mg Castings B443.0 Castings A356.0 A13560 A05350 A97005 209 19/12 [130/83] Al-4Mg-Zn A24430 Al-Si 23/13 [160/90] A13560 Al-7Mg-Mn 25/14 [170/97] 7020, T5 [130/–] 19/– Castings 17/7 [115/48] A97020 Al-7Si Castings 22/9 Al-Si Castings 34/24 [235/165] 35/18 [240/125] Castings [–/–] –/– 17/6 [115/41] Castings [160/–] 23/– Al-3Si-4Cu Castings Castings Al-8Si-1Cu-Mn-Mg Shapes& Rod, Al-6Si-3Cu Bar, Castings [275/–] 40/– Castings Al-Si-Mg Al-Zn-Mg-Mn-Cr-Ti Shapes, Rod, & Tube Bar, Al-4.5Zn-1.2Mg-Mn-Cr-Zr Al-Si Al-7Mg-Mn Al-Si-Mg Al-Si Al-Si-Mg Material Number
163 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition ate, Sheet, Strip, & Barate, Sheet, 99.99Cu-P [205/62][205/62][205/62] Seamless Pipe[205/62] Seamless Pipe[205/62] Seamless Pipe Seamless Pipe Seamless Pipe 99.95Cu-P 99.95Cu-P 99.95Cu-P 99.9Cu-P 99.9Cu-P [205/62][205/62][205/62] Seamless Tube[205/62] Seamless Tube Seamless Tube Seamless Tube[205/62] 99.99Cu-P 99.95Cu-P Seamless Tube 99.95Cu-P 99.95Cu-P 99.4Cu-As-P 9 [205/62]9 [205/62] Seamless Tube Seamless Tube 99.9Cu-P 99.9Cu-P 9 [205/62]9 [205/62] Seamless Tube Seamless Tube 99.9Cu-P 99.9Cu-P Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc .2 [mm] Diameter Diameter Thickness or (Continued) Limitations, in in Limitations, Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 3131 3131 3131 ASTM/ASME 3131 ASTM/ASME B/SB-42 3131 ASTM/ASME B/SB-42 3131 ASTM/ASME B/SB-42 3131 ASTM/ASME — B/SB-42 3131 — B/SB-42 3131 ASTM — 3131 C10200 ASTM — 3131 C10300 ASTM — 3131 C10800 ASTM B68 3131 ASTM/ASME C12000 ASTM B68 3131 ASTM/ASME C12200 B68 B/SB-75 3131 ASTM/ASME B68 B/SB-75 31 —31 ASTM/ASME B68 B/SB-75 31 —31 ASTM/ASME 30/9 — B/SB-75 31 —31 ASTM/ASME 30/9 — B/SB-75 C10200 31 —31 ASTM/ASME 30/9 — B/SB-75 C10300 31 —31 C10100 30/9 — B/SB-75 C10800 3131 C10200 ASTM 30/9 — C12000 3131 C10300 ASTM — C12200 3131 ASTM/ASME C10800 ASTM — 3131 ASTM/ASME C12000 B88 B/SB-111 3131 ASTM/ASME C12200 B88 B/SB-111 30/9 [205/62] 3131 ASTM/ASME C14200 B88 B/SB-111 30/9 [205/62] 3131 — ASTM/ASME 30/9 [205/62] B/SB-111 30/9 [205/62] 31 —31 — ASTM/ASME 30/9 [205/62] B/SB-111 30/9 [205/62] 31 — — ASTM/ASME 30/9 [205/62] B/SB-111 30/9 [205/62] 31 C10100 — Tube — ASTM/ASME Seamless Tube 30/9 [205/62] B/SB-111 C10200 C10200 Tube — Seamless ASTM/ASMETube 30/ B/SB-111 C12000 C10300 Tube — Seamless Tube 30/ B/SB-152 C12200 C10800 Tube — Seamless Tube 30/9 [205/62] C12000 Tube — 99.99Cu-P C12200 — 99.95Cu-P C14200 99.95Cu-P Seamless Tube 99.95Cu-P C19200 99.95Cu-P 30/9 99.95Cu-P C10100 [205/–] 30/– 99.95Cu-P 30/9 [205/–] 30/– 30/9 99.9Cu-P [205/–] 30/– 30/9 99.9Cu-P 99.40Cu-P 30/ 30/ Tube 30/9 Tube 38/12 [260/83] Tube 30/9 [205/62] Pl Seamless Tube 99.95Cu-P 99.9Cu-P 99.9Cu-P 99.7Cu-Fe-P Material Number
164 AWS B2.1/B2.1M-BMG:2014 & Bar 99.4Cu-As-P & Bar & Bar & BarAg + 99.95Cu Ag + 99.95Cu Ag + 99.95Cu p, & Bar 99.9Cu-P p, & Barp, & Bar 99.9Cu-P 99.9Cu-P rip, & Bar 99.90Cu t Form Nominal Composition e, Sheet, Strip, & Bare, Sheet, 99.99Cu-Sn-Te ate, Sheet, Stri ate, Sheet, ate, Sheet, Stri ate, Sheet, Stri ate, Sheet, Strip, ate, Sheet, ate, Sheet, Strip, & Barate, Sheet, Strip, & Barate, Sheet, Strip, ate, Sheet, Strip, ate, Sheet, 99.95Cu-P Strip, ate, Sheet, 99.95Cu-P Strip, & Barate, Sheet, 99.95Cu-P Plate, Sheet, St Plate, Sheet, [195/55] Rod & Bar 99.99Cu-Sn-Te 8 [195/55]8 [195/55]8 [195/55] Rod & Bar Rod & Bar Rod & Bar 99.95Cu + Ag 99.95Cu + Ag 99.90Cu + Ag Minimum Minimum Tensile/Yield Tensile/Yield 28/8 [195/55] Rod & Bar 99.9Cu Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 31 31 ASTM/ASME B/SB-152 — C12000 30/9 [205/62] Pl 31 31 ASTM/ASME31 B/SB-15231 3131 3131 — 3131 ASTM 3131 ASTM/ASME ASTM 31 C1220031 ASTM/ASME B/SB-187 3131 B170 ASTM/ASME B/SB-187 3131 B170 ASTM/ASME B/SB-187 3131 — ASTM/ASME B/SB-187 3131 — ASTM/ASME B/SB-187 1 3131 — ASTM/ASME B/SB-187 2 31 C1010031 — ASTM/ASME B/SB-187 31 C1020031 30/9 [205/62] — B/SB-187 C10100 31 C1030031 — ASTM Pl C10200 31 C1040031 — ASTM 31 C1070031 — ASTM 31 C10940 B280 ASTM 31 C11000 B280 ASTM C14420 28/8 [195/55] B280 ASTM 28/8 [195/55] B302 ASTM 102 30/9 [205/62] 28/8 [195/55] B302 120 30/9 [205/62] 28/ B359 122 Rod & Bar C10200 28/ B359 Rod & Bar — C12000 28/ Rod & Bar — Shapes C12200 — Shapes 28/8 C12000 — C12200 99.99Cu-P C10100 99.95Cu-P C10200 99.95Cu-P [205/–] 30/– 99.99Cu-P [205/–] 30/– 99.95Cu-P [205/–] 30/– Seamless Tube 30/9 [205/62] Seamless Tube 30/9 [205/62] Seamless Tube 30/9 [205/62] 30/9 [205/62] Pipe 99.95Cu-P Seamless Tube Pipe 99.9Cu-P Seamless Tube 99.9Cu-P 99.99Cu-P 99.95Cu-P 99.9Cu-P 99.9Cu-P 31 31 ASTM/ASME B/SB-152 — C14420 30/9 [205/62] Plat 3131 31 31 ASTM/ASME ASTM/ASME B/SB-152 B/SB-152 — — C12300 C14200 30/9 [205/62] 30/9 [205/62] Pl Pl 31 31 ASTM/ASME B/SB-152 — C10200 30/9 [205/62] Pl 3131 3131 3131 ASTM/ASME 3131 ASTM/ASME B/SB-152 3131 ASTM/ASME B/SB-152 31 ASTM/ASME B/SB-152 31 — ASTM/ASME B/SB-152 — ASTM/ASME B/SB-152 — B/SB-152 C10300 — C10400 — C10500 — C10700 C10800 C11000 30/9 [205/62] 30/9 [205/62] Pl 30/9 [205/62] Pl 30/9 [205/62] Pl 30/9 [205/62] Pl 30/9 [205/62] Pl Material Number
165 AWS B2.1/B2.1M-BMG:2014 u-28Zn-1Sn-0.06Sb t Form Nominal Composition 105] Seamless Tube 71Cu-28Zn-1Sn-0.06As 310/105] Seamless Tube 71C 310/105] Seamless Tube 71Cu-28Zn-1Sn-0.06P [205/62][205/62][205/62] Seamless Tube Seamless Tube Seamless Tube[205/62] 99.95Cu-P Seamless Tube 99.95Cu-P 99.95Cu-P 99.4Cu-As-P [345/125] Seamless Tube 78Cu-20Zn-2Al 9 [205/62] Seamless Tube9 [205/62]9 [205/62] 99.9Cu-P Seamless Tube Seamless Tube 99.9Cu-P 99.9Cu-P 12 [275/83]12 [275/83] Pipe Seamless Seamless Tube 85Cu-15Zn 85Cu-15Zn 12 [260/83] Seamless Tube 90Cu-10Zn Minimum Minimum Tensile/Yield Tensile/Yield 52/20 [360/140] Rod & Bar 60Cu-39Zn-Sn Strength, ksi [MPa] Produc 2 50] ≤ ≤ 25] 54/20 [370/140] Rod & Bar 60Cu-39Zn-Sn ≤ [mm] 1 [ ≤ Diameter Diameter .2 (Continued) Thickness or [>25 and [>25 and (Continued) Limitations, in in Limitations, Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 3131 3131 3131 31 ASTM 31 ASTM ASTM/ASME ASTM B359 B/SB-359 B359 B359 — — — — C12200 C10300 C10800 C12000 30/ 30/9 [205/62] 30/9 [205/62] 30/9 [205/62] Seamless Tube Seamless Tube Seamless Tube 99.95Cu-P 99.95Cu-P 99.9Cu-P 3131 3131 3131 3131 ASTM 3131 ASTM/ASME ASTM 3131 ASTM/ASME B/SB-395 3131 B359 ASTM/ASME B/SB-395 3131 B359 ASTM/ASME B/SB-395 3131 — ASTM/ASME B/SB-395 3131 — ASTM/ASME B/SB-395 — 3131 — ASTM/ASME B/SB-395 — 31 C1020032 — ASTM/ASME B/SB-395 31 C1030032 — ASTM/ASME C14200 B/SB-543 32.2 C10800 — ASTM/ASME C19200 B/SB-543 32.232 C12000 — B/SB-54332 ASTM C12200 — 32.232 ASTM C14200 — 32.232 C19200 — 32.1 ASTM32 B21 C10800 30/9 32.1 ASTM/ASME ASTM32 B21 C12200 30/9 32.1 30/9 [205/62] ASTM/ASME32 B/SB-43 C19400 30/9 38/12 [260/83] 32.2 ASTM/ASME B21 B/SB-111 30/ 32.2 — ASTM/ASME B21 B/SB-111 30/ Seamless Tube — ASTM/ASME B/SB-111 — Seamless Tube 30/9 — B/SB-111 38/12 [260/83] C46400 — — 30/9 [205/62] C46400 — — C23000 30/9 [205/62] C23000 — Seamless Tube 45/15 [310/105] C46400 99.40Cu-P C28000 >1 and 99.7Cu-Fe-P C46400 Tube Welded C44300 Tube Welded C44400 >2 [>50] Tube Welded 99.7Cu-Fe-P 52/20 [360/140] 50/20 [345/140] 40/ 99.95Cu-P 40/ 50/20 [345/140] 99.9Cu-P Rod & Bar 97.5Cu-P Shapes 45/15 [310/ 45/15 [ Seamless Tube 60Cu-39Zn-Sn 60Cu-39Zn-Sn 60Cu-40Zn 3232 32.232 32.2 ASTM/ASME 32.1 ASTM/ASME B/SB-111 ASTM/ASME B/SB-111 B/SB-135 — — — C44500 C68700 C22000 45/15 [ 50/18 38/ Material Number
166 AWS B2.1/B2.1M-BMG:2014 u-28Zn-1Sn-0.06Sb u-28Zn-1Sn-0.06Sb r 98.5Cu-3Si-1.5Sn-Cr & Bar 98.5Cu-1.5Si t Form Nominal Composition Sheet, Strip, & Ba Sheet, ate, Sheet, Strip, ate, Sheet, Strip, & Barate, Sheet, 97Cu-3Si ] Seamless Pipe & Tube 98.5Cu-1.5Si 105]105]105] Plate & Sheet Plate & Sheet Plate & Sheet 71Cu-28Zn-1Sn-0.06As 105] 71Cu-28Zn-1Sn-0.06Sb 71Cu-28Zn-1Sn-0.06P Seamless Tube 71Cu-28Zn-1Sn-0.06As 105] Seamless Tube 71Cu-28Zn-1Sn-0.06As 310/105] Seamless Tube 71C 310/105] Seamless Tube310/105]310/105] 71Cu-28Zn-1Sn-0.06P Seamless Tube Seamless Tube310/105] 71C 71Cu-28Zn-1Sn-0.06P Tube Welded 71Cu-28Zn-1Sn-0.06Sb [345/125][345/125] Plate & Sheet Plate & Sheet 60Cu-39Zn-Sn 60Cu-39Zn-As [345/125] Seamless Tube 78Cu-20Zn-2Al 12 [275/83] Seamless Tube 85Cu-15Zn 12 [275/83] Seamless Tube 85Cu-15Zn Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 32 32.1 ASTM/ASME B/SB-135 — C23000 40/ 3232 32.232 32.2 ASTM/ASME32 32.2 ASTM/ASME B/SB-17132 32.2 ASTM/ASME B/SB-17132 32.2 ASTM/ASME B/SB-17132 32.1 — ASTM/ASME B/SB-17132 32.2 — B/SB-171 32.2 — ASTM/ASME ASTM C44300 — ASTM/ASME B/SB-359 C44400 — B/SB-359 C44500 B359 C46400 — C46500 — — C44300 45/15 [310/ C44400 45/15 [310/ C23000 45/15 [310/ 50/18 50/18 45/15 [310/ 45/15 [ 40/12 [275/83] Seamless Tube 85Cu-15Zn 3232 32.232 32.2 ASTM/ASME32 32.1 B/SB-35932 32.2 ASTM/ASME ASTM32 32.2 ASTM/ASME B/SB-39532 32.2 — ASTM/ASME B/SB-39532 32.2 B359 ASTM/ASME B/SB-39532 32.1 — ASTM/ASME B/SB-39532 C44500 32.2 — ASTM/ASME B/SB-39532 32.2 — ASTM/ASME B/SB-54332 — C23000 32.2 — ASTM/ASME B/SB-54333 C44300 32.2 — ASTM/ASME B/SB-543 C44400 — ASTM/ASME C68700 37 B/SB-543 C44500 — B/SB-543 ASTM/ASME C68700 — 45/15 [ C23000 B/SB-96 — C44300 — 40/ C44400 45/15 [310/ C44500 — 45/15 [ C68700 50/18 [345/125] 45/15 [ 50/18 C65100 Seamless Tube 40/12 [275/83] 45/15 [310/105] 45/15 [ Tube 45/15 [310/105] Welded Tube Welded 78Cu-20Zn-2Al 50/18 [345/125] Tube Welded [260/–] 38/– Tube 71Cu-28Zn-1Sn-0.06As Welded 85Cu-15Zn Pl 71Cu-28Zn-1Sn-0.06P 78Cu-20Zn-2Al 33 373333 ASTM/ASME 3733 B/SB-96 3733 ASTM/ASME 3733 ASTM/ASME B/SB-98 31 ASTM/ASME — B/SB-98 37 ASTM/ASME B/SB-98 ASTM/ASME B/SB-283 — C65400 B/SB-315 — — — C65100 — C65500 C66100 C65500 C65100 [450/–] 65/– Plate, 40/12 [275/83] 52/15 [360/105] 52/15 [360/105] & Shapes Bar, Rod, 50/15 [345/105] & Shapes Bar, Rod, & Shapes Bar, Rod, 40/10 [275/69 98.5Cu-1.5Si Forgings 97Cu-3Si 94Cu-3Si 97Cu-3Si 33 37 ASTM/ASME B/SB-96 — C65500 50/18 [345/125] Pl Material Number
167 AWS B2.1/B2.1M-BMG:2014 5Cu-10Ni-Fe-Mn t Form Nominal Composition amless Tube 80Cu-16Ni-0.75Fe-0.5Cr 110] Seamless Tube 80Cu-16Ni-0.75Fe-0.5Cr 110] Seamless Tube 80Cu-16Ni-0.75Fe-0.5Cr 345/105] Seamless Pipe & Tube435/170] 97Cu-3Si Seamless Tube 66Cu-30Ni-2Fe-2Mn [310/170] Castings 87. 15 [275/105]16 [310/110]18 [360/125] Seamless Tube Seamless Tube Seamless Tube15 [260/105] 90Cu-10Ni Rod & Bar 80Cu-20Ni 70Cu-30Ni 90Cu-10Ni 15 [275/105]16 [310/110]18 [360/125] Seamless Tube Seamless Tube Seamless Tube 90Cu-10Ni 80Cu-20Ni 70Cu-30Ni 15 [275/105]16 [310/110]18 [360/125] Seamless Tube Seamless Tube Seamless Tube 90Cu-10Ni 80Cu-20Ni 70Cu-30Ni Minimum Minimum Tensile/Yield Tensile/Yield 48/18 [330/125] Oct)Hex, (Rnd, Rod & Bar Sq 70Cu-30Ni 45/18 [310/125]45/18 Plate & Sheet 70Cu-30Ni Strength, ksi [MPa] Produc 1 5 25] ≤ ≤ 127] ≤ 13] 52/18 [360/125] Oct)Hex, (Rnd, Rod & Bar Sq 70Cu-30Ni 64][345/140] 50/20 Plate & Sheet 70Cu-30Ni 64][290/110] 42/16 Plate & Sheet 80Cu-16Ni-0.75Fe-0.5Cr ≤ ≤ ≤ ≤ [mm] 0.5 [ 2.5 [ 2.5 [ Diameter Diameter ≤ ≤ ≤ .2 (Continued) Thickness or [>13 and [>13 and (Continued) Limitations, in in Limitations, [>64 and Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 3434 3434 3434 ASTM/ASME 3434 ASTM/ASME B/SB-111 3434 ASTM/ASME B/SB-111 3434 ASTM/ASME B/SB-111 3434 — ASTM/ASME B/SB-111 3434 — ASTM/ASME B/SB-111 34 — ASTM/ASME B/SB-111 34 C70400 — ASTM/ASME B/SB-151 C70600 — ASTM/ASME B/SB-15134 C71000 — B/SB-15134 C71500 — 34 C71640 — 34 C72200 ASTM/ASME — C70600 ASTM/ASME B/SB-171 38/12 [260/83] C71500 B/SB-171 40/ C71500 45/ — Seamless Tube 52/ — 63/25 [ C70600 45/16 [310/ C71500 38/ [310/105] 45/15 95Cu-5Ni & Shapes Bar (Rect.) [275/105] 40/15 70Cu-30Ni Plate & Sheet 90Cu-10Ni 33 33 ASTM/ASME B/SB-315 — C65500 50/15 [ 3434 34 34 ASTM/ASME ASTM/ASME B/SB-15134 B/SB-151 34 — ASTM/ASME — B/SB-171 C71500 C71500 — >1 [>25] >0.5 and 45/18 [310/125] Oct)Hex, (Rnd, C71500 Rod & Bar Sq >2.5 and 70Cu-30Ni 34 34 ASTM/ASME B/SB-171 — C72200 3434 3434 3434 3434 ASTM/ASME ASTM 3434 ASTM/ASME B/SB-359 34 ASTM/ASME B/SB-359 34 B359 B/SB-359 — ASTM/ASME ASTM — B/SB-369 — — C70600 B359 C71000 — C71500 C70400 — C96200 C72200 40/ 45/ 52/ 38/12 [260/83] 45/25 Seamless Tube 45/16 [310/110] Se 95Cu-5Ni 3434 3434 3434 ASTM/ASME 3434 ASTM/ASME B/SB-395 34 ASTM/ASME B/SB-395 34 ASTM/ASME B/SB-395 — ASTM/ASME B/SB-395 — B/SB-395 — C70400 — C70600 — C71000 C71500 C72200 38/12 [260/83] 40/ 45/ Seamless Tube 52/ 45/16 [310/ 95Cu-5Ni Material Number
168 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition mless Pipe & Tube 80Cu-16Ni-0.75Fe-0.5Cr 83]90] Seamless Pipe & Tube Seamless Pipe & Tube 95Cu-5Ni 90Cu-10Ni 275] Castings 75Cu-8Al-3Fe-2-Ni-12Mn 485/205] Seamless Tube515/205] 90Cu-7Al-2.5Fe-Sn Castings 84Cu-10Al-4Fe-2Ni 310/110]360/125] Seamless Pipe & Tube Seamless Pipe & Tube 80Cu-20Ni 70Cu-30Ni [485/205] Seamless Tube[620/275] 90Cu-7Al-3Fe Castings 82Cu-11Al-4Fe-3Mn 19 [345/130] Seamless Tube25 [450/170]25 [450/170]30 [515/205] Castings 95Cu-5Al Castings28 [415/195] Castings Castings 88Cu-9Al-3Fe 89Cu-10Al-1Fe 85Cu-11Al-4Fe 90Cu-7Al-3Si Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc 114] 38/13 [260/90] Pipe Welded 90Cu-10Ni 114] 40/15 [275/105]114] 50/20 [345/140] Pipe Welded Pipe Welded 90Cu-10Ni 70Cu-30Ni ≤ ≤ [mm] 4.5 [ 4.5 [ Diameter Diameter ≤ ≤ .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 3434 3434 3434 ASTM/ASME 3434 ASTM/ASME B/SB-467 3434 ASTM/ASME B/SB-467 3434 ASTM/ASME B/SB-467 3434 — ASTM/ASME B/SB-467 3434 — ASTM/ASME B/SB-543 3434 — B/SB-543 34 C7060034 — ASTM/ASME ASTM 34 C70600 34 — ASTM/ASME B/SB-543 >4.5 [> 34 C7150034 — B/SB-543 34 C71500 34 B543 ASTM >4.5 [>114] 34 C7040035 — ASTM 34 C7060035 — ASTM/ASME ASTM 45/15 [310/105] 3535 B543 ASTM/ASME B/SB-956 — 35 C7150035 B608 ASTM/ASME B/SB-956 35 C7164035 Pipe Welded B608 ASTM/ASME B/SB-111 3535 — ASTM/ASME C71000 B/SB-111 — 3535 — ASTM/ASME B/SB-111 — 35 38/12 [260/83]35 — ASTM/ASME B/SB-148 — 40/15 [275/105] 35 C7060035 — ASTM/ASME C72200 B/SB-148 35 C7150035 70Cu-30Ni — ASTM/ASME C70620 B/SB-148 Tube 52/18 [360/125] Welded 35 C60800 — ASTM/ASME C71520 Tube Welded B/SB-148 63/25 [435/170] 35 C61300 — ASTM/ASME B/SB-148 C61400 45/16 [310/110] — ASTM/ASME Tube Welded B/SB-148 C95200 — Tube Welded B/SB-148 C95300 — 95Cu-5Ni 40/15 [275/105] Tube Welded C95400 45/16 [310/110] 90Cu-10Ni — 52/18 [360/125] C95410 — Tube Welded Finned [275/–] 40/– 50/ 66Cu-30Ni-2Fe-2Mn C95500 70Cu-30Ni Tube Welded Finned [345/–] 50/– 70/30 [ Tube Welded C95600 70/30 C95700 80Cu-20Ni 65/ Pipe Welded 90Cu-10Ni 80Cu-16Ni-0.75Fe-0.5Cr 65/ Pipe Welded 70Cu-30Ni 75/ 75/30 [ 90/40 87Cu-10Ni-1.4Fe 60/ 65Cu-31Ni-0.7Fe 90/40 [620/ 3434 3434 3434 ASTM/ASME 34 ASTM/ASME B/SB-466 34 ASTM/ASME B/SB-466 ASTM/ASME B/SB-466 — B/SB-466 — — C70600 — C71000 C71500 C72200 38/13 [260/ 45/16 [ 52/18 [ 40/14 [275/97] Sea 34 34 ASTM/ASME B/SB-466 — C70400 37/12 [255/ Material Number
169 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition 240] Castings 81Cu-9Al-4.5Ni-4Fe-1.2Mn Minimum Minimum Tensile/Yield Tensile/Yield 75/35 [515/240]75/35 [485/205]70/30 Bar & Rod[485/220]70/32 Bar & Rod88/44 [605/305] Bar & Rod 90Cu-7Al-3Fe Rod (Round) 90Cu-7Al-3Fe 90Cu-7Al-3Fe 87Cu-9Al-4Fe 88/44 [605/305] Rod (Round) 88Cu-9Al-3Fe 75/45 [515/310] Rod (Round)[515/240]75/35 Oct)& (Hex Bar & Rod 72/40 [495/275] 90Cu-7Al-2.5Fe-Sn 90Cu-7Al-2.5Fe-Sn Rod (Round) 90Cu-7Al-2.5Fe-Sn 85/40 [585/275] Rod (Round)78/37 [540/255] Rod (Round) 87Cu-9Al-4Fe 87Cu-9Al-4Fe 70/35 [485/240][485/220]70/32 Rod (Round)Oct)& (Hex Bar & Rod 90Cu-7Al-2.5Fe-Sn 90Cu-7Al-2.5Fe-Sn Strength, ksi [MPa] Produc 1 1 1 1 1 25] 3 75] 2 50] 25] 25] 25] 25] 2 50] 2 50] 3 75] 3 75] 2 50] ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ 13][550/275] 80/40 13] 90/50 [620/345] Bar & Rod Rod (Round) 90Cu-7Al-3Fe 87Cu-9Al-4Fe 13][550/275] 80/40 Oct)& (Hex Bar & Rod 90Cu-7Al-2.5Fe-Sn 13] 80/50 [550/345] Rod (Round) 90Cu-7Al-2.5Fe-Sn ≤ ≤ ≤ ≤ [mm] 0.5 [ 0.5 [ 0.5 [ 0.5 [ Diameter Diameter ≤ ≤ ≤ ≤ .2 (Continued) Thickness or [>13 and [>13 and [>50 and [>25 and [>13 and [>13 and [>13 and [>13 and [>13 and [>25 and [>25 and [>50 and [>50 and [>50 and [>25 and (Continued) Limitations, in in Limitations, Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 3535 35 ASTM/ASME35 35 B/SB-150 ASTM/ASME 35 B/SB-15035 ASTM/ASME — B/SB-150 35 — ASTM/ASME C61400 B/SB-150 — C61400 >2 and C61400 — >1 and C61900 35 35 ASTM/ASME B/SB-15035 — 3535 ASTM/ASME C61300 B/SB-15035 35 ASTM/ASME 35 B/SB-150 — ASTM/ASME B/SB-150 C61300 —35 — C61300 3535 ASTM/ASME C61400 >1 and B/SB-15035 35 >0.5 and 35 ASTM/ASME 3535 B/SB-150 — 35 ASTM/ASME 35 ASTM/ASME B/SB-150 ASTM/ASME C61900 B/SB-150 — B/SB-150 — >0.5 and C61900 — — C61900 >1 and C61900 C61900 >3 [>75] >2 and 75/30 [515/205] Rod (Round) 75/30 [515/205] Shapes 87Cu-9Al-4Fe 87Cu-9Al-4Fe 35 35 ASTM/ASME B/SB-148 — C95800 85/35 [585/ 35 35 ASTM/ASME B/SB-150 — C62300 >0.5 and 3535 35 ASTM/ASME35 35 B/SB-150 ASTM/ASME 35 B/SB-15035 ASTM/ASME — B/SB-150 35 — ASTM/ASME C61300 B/SB-150 — C61300 >2 and C61300 — >1 and >0.5 and C61300 >0.5 and Material Number
170 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition 515/205]Oct)& (Hex Bar & Rod 88Cu-9Al-3Fe 40 [550/275]40 Bar & Rod 81Cu-10Al-5Ni-3Fe Minimum Minimum Tensile/Yield Tensile/Yield 76/37 [525/255] Rod (Round)84/40 [580/275][540/220]78/32 Rod (Round)Oct)& (Hex Bar & Rod 88Cu-9Al-3Fe 88Cu-9Al-3Fe 88Cu-9Al-3Fe 90/35 [620/240]90/40 [620/275] Rod (Round)90/43 [620/295] Rod (Round) Rod (Round) 87Cu-10Al-3Fe 87Cu-10Al-3Fe 87Cu-10Al-3Fe 90/35 [620/240] & Oct) & Rod (Hex Bar, 87Cu-10Al-3Fe [620/310]90/45 Bar & Rod 81Cu-10Al-5Ni-3Fe 130/95 [895/655]130/95 Bar & Rod 80Cu-10Al-5Ni-5Fe 100/50 [690/345]100/50 Bar & Rod 81Cu-10Al-5Ni-3Fe 85/42.5 [585/295] 85/42.5 Bar & Rod 81Cu-10Al-5Ni-3Fe Strength, ksi [MPa] Produc 5 1 3 75] 2 50] 2 50] 5 3 75] 2 50] 50] 2 50] 4 2 25] ≤ ≤ 125] 125] 100] ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ 13] 90/50 [620/345] Rod (Round) 88Cu-9Al-3Fe ≤ ≤ ≤ 25][550/240] 80/35 Oct)& (Hex Bar & Rod 88Cu-9Al-3Fe 25] 95/45 [655/310] Rod (Round) 87Cu-10Al-3Fe ≤ ≤ ≤ [mm] 1 [ 1 [ 0.5 [ ≤ ≤ 0.5 and 0.5 and Diameter Diameter 13 and 13 ≤ ≥ .2 (Continued) ≥ Thickness or [ [>50 and [>50 and [>25 and [>25 and [>50 and [>50 and [>25 and [>25 and [>25 and [>25 and [>25 and (Continued) Limitations, in in Limitations, [>75 and [>13 and [>50 and Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 3535 3535 35 ASTM/ASME35 35 ASTM/ASME B/SB-15035 ASTM/ASME B/SB-150 35 B/SB-15035 35 ASTM/ASME — ASTM/ASME B/SB-150 —35 35 B/SB-150 — ASTM/ASME C62300 35 C62300 B/SB-150 — ASTM/ASME C62300 — B/SB-150 C62300 — >2 and C62300 — >3 [>75] C62300 75/30 [515/205] >1 and 75/30 [515/205] C62300 >1 and Shapes Rod (Round) 88Cu-9Al-3Fe 88Cu-9Al-3Fe 35 35 ASTM/ASME B/SB-150 — C62300 >2 [>50] 75/30 [ 3535 35 35 ASTM/ASME ASTM/ASME B/SB-150 B/SB-150 — — C62400 C62400 >3 and 90/35 [620/240] Shapes 87Cu-10Al-3Fe 3535 35 ASTM/ASME35 35 B/SB-150 ASTM/ASME 35 B/SB-150 ASTM/ASME — B/SB-150 — C62400 — C62400 >2 and C62400 >1 and >0.5 and 3535 3535 35 ASTM/ASME35 35 ASTM/ASME B/SB-150 ASTM/ASME B/SB-15035 35 B/SB-150 ASTM/ASME — 35 B/SB-150 — ASTM/ASME — C62400 B/SB-150 C63000 — C63000 — C63000 C63000 >1 and [585/295] 85/42.5 >2 and Shapes 81Cu-10Al-5Ni-3Fe 3535 35 35 ASTM/ASME ASTM/ASME B/SB-150 B/SB-150 — — C63000 C63020 >4 [>100] >1 and 80/ Material Number
171 AWS B2.1/B2.1M-BMG:2014 eeteet 90Cu-7Al-2.5Fe-Sn 90Cu-7Al-2.5Fe-Sn Sheet 90Cu-7Al-2.5Fe-Sn Strip, & BarStrip, & Bar 90Cu-7Al-3Fe Strip, & Bar 90Cu-7Al-3Fe 90Cu-7Al-3Fe t Form Nominal Composition eet, Strip, & Bareet, 90Cu-7Al-2.5Fe-Sn eet, Strip, & Bareet, 90Cu-7Al-2.5Fe-Sn Sheet, Strip, & BarSheet, 90Cu-7Al-2.5Fe-Sn Minimum Minimum Tensile/Yield Tensile/Yield 85/45 [585/310]85/45 [485/170]70/25 Bar & Rod Bar & Rod 91Cu-7Al-2Si 91Cu-7Al-2Si 70/30 [485/205]70/30 [515/240]75/35 Bar & Rod[550/290]80/42 Bar & Rod Bar & Rod 91Cu-7Al-2Si 72/32 [485/220] 91Cu-7Al-2Si Plate, Sh 91Cu-7Al-2Si 65/28 [450/195] Plate, Sheet, 70/30 [485/205] Plate, Sheet, 70/30 [485/205]70/30 Plate & Sh [450/195]65/28 Plate & Sh 65/28 [450/195] Plate, Sh 130/90 [895/620]130/90 Bar & Rod 80Cu-10Al-5Ni-5Fe Strength, ksi [MPa] Produc 1 2 2 25] 4 5 4 3 75] 2 50] 51] 51] 5 5 3 80] ≤ ≤ ≤ 100] 127] 100] 130] 127] ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ 13] 75/36 [515/250] Plate, 13][620/310] 90/45 Bar & Rod 91Cu-7Al-2Si 13] 72/32 [495/220] Plate, Sheet, ≤ ≤ ≤ ≤ ≤ 51][485/195] 70/28 Plate & Sheet 90Cu-7Al-3Fe 25] [930/690] 135/100 Bar & Rod 80Cu-10Al-5Ni-5Fe 50] 75/37 [515/255] Plate & ≤ ≤ ≤ ≤ ≤ ≤ [mm] 2 [ 1 [ 2 [ 0.5 [ 0.5 [ 0.5 [ ≤ ≤ ≤ Diameter Diameter ≤ ≤ ≤ .2 (Continued) Thickness or [>13 and [>13 and [>50 and [>50 and [>25 and [>13 and [>13 and [>50 and [>50 and (Continued) Limitations, in in Limitations, [>75 and [>51 and [>50 and [>80 and [>51 and Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 35 35 ASTM/ASME B/SB-171 — C61400 3535 35 35 ASTM/ASME ASTM/ASME B/SB-150 B/SB-150 — — C64200 C6420035 >4 [>100] 35 >3 and 35 35 ASTM/ASME ASTM/ASME B/SB-169 B/SB-169 — — C61300 C61400 >2 and 35 35 ASTM/ASME B/SB-150 — C63020 >2 and 35 35 ASTM/ASME B/SB-171 — C61300 3535 3535 35 ASTM/ASME 35 ASTM/ASME B/SB-150 ASTM/ASME B/SB-150 B/SB-15035 — —35 35 — ASTM/ASME C63020 35 35 C63200 B/SB-15035 ASTM/ASME C64200 35 B/SB-150 35 ASTM/ASME — >0.5 and ASTM/ASME B/SB-150 — B/SB-150 C64200 — 90/40 [620/275] C64200 — >2 and & ShapesRod, Bar, C64200 >1 and C64200 83Cu-9Al-4Ni-4Fe 35 35 70/30 [485/205] ASTM/ASME B/SB-171 Shapes — C61300 91Cu-7Al-2Si >3 and 3535 35 ASTM/ASME 35 B/SB-169 ASTM/ASME B/SB-16935 —35 35 —35 ASTM/ASME C61300 35 B/SB-169 35 ASTM/ASME C61300 >2 and ASTM/ASME B/SB-169 B/SB-171 — >0.5 and — C61400 — C61400 >0.5 and C61300 >2 and Material Number
172 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition Seamless Pipe & Tube 90Cu-7Al-2.5Fe-Sn 195] Seamless Pipe & Tube 90Cu-7Al-3Fe 515/205] Castings 84Cu-10Al-4Fe-2Ni [620/275] Castings 82Cu-11Al-4Fe-3Mn 25 [450/170]25 [450/170]30 [515/205] Castings Castings Castings 88Cu-9Al-3Fe 89Cu-10Al-1Fe 19 [345/130] 85Cu-11Al-4Fe 26 [470/180] Seamless Tube Castings 95Cu-5Al 88Cu-9Al-3Fe Minimum Minimum Tensile/Yield Tensile/Yield 85/33 [585/230]85/33 Plate & Sheet 81Cu-10Al-5Ni-3Fe 65/26 [450/180]65/26 Plate & Sheet[550/205]80/30 90Cu-7Al-3Fe Plate & Sheet[585/230]85/33 81Cu-10Al-5Ni-3Fe Plate & Sheet 83Cu-9Al-4Ni-4Fe 80/30 [550/205]80/30 Plate & Sheet 83Cu-9Al-4Ni-4Fe Strength, ksi [MPa] Produc 5 5 89] 5 89] ≤ ≤ 127] 127] 127] 3.5 3.5 ≤ ≤ ≤ 40] 68/23 [470/160] Forgings 91Cu-7Al-2Si 40] 70/25 [485/170] Forgings 91Cu-7Al-2Si ≤ ≤ ≤ ≤ ≤ 51][620/250] 90/36 Plate & Sheet 81Cu-10Al-5Ni-3Fe 51][620/250] 90/36 Plate & Sheet 83Cu-9Al-4Ni-4Fe ≤ ≤ ≤ [mm] 2 [ 2 [ 1.5 [ ≤ ≤ Diameter Diameter ≤ .2 (Continued) Thickness or [>51 and [>51 and [>51 and [>51 and Limitations, in in Limitations, [>51 and [>89 and [>89 and Table C Copper and Copper Base Alloys Base Copper and Copper UNS Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 35 35 ASTM/ASME B/SB-171 — C63000 >3.5 and 35 35 ASTM/ASME B/SB-171 — C61400 >2 and 3535 35 35 ASTM/ASME ASTM/ASME B/SB-17135 B/SB-171 35 — ASTM/ASME — B/SB-17135 C63000 35 C63000 3535 — 3535 ASTM/ASME >2 and 3535 ASTM/ASME B/SB-271 3535 ASTM/ASME C63200 B/SB-271 3535 ASTM/ASME B/SB-271 35 — ASTM/ASME >3.5 and B/SB-271 3535 — ASTM/ASME B/SB-27135 — ASTM/ASME B/SB-283 35 C9520035 — B/SB-283 35 C9530035 — ASTM/ASME 35 C9540035 — B/SB-315 35 C9541035 — ASTM/ASME ASTM 35 C95500 ASTM/ASME B/SB-395 35 C64200 — B/SB-505 C64200 B359 ASTM 65/ >1.5 [> — ASTM 65/ C61400 — 75/ B608 — 75/30 [ C60800 B608 90/40 C95200 C60800 — — 65/28 [450/ C61300 C61400 50/ 68/ 50/19 [345/130] Seamless Tube [485/–] 70/– [485/–] 70/– Pipe Welded 95Cu-5Al Pipe Welded 90Cu-7Al-2.5Fe-Sn 90Cu-7Al-3Fe 35 35 ASTM/ASME B/SB-315 — C61300 65/28 [450/195] 3535 35 35 ASTM/ASME ASTM/ASME B/SB-171 B/SB-171 — — C63200 C63200 >2 and Material Number
173 AWS B2.1/B2.1M-BMG:2014 Tube C 99.0Ni-Low & Strip 99.0Ni pe, Tube 99.0Ni t Form Nominal Composition Bar, & Wire Bar, 63Ni-25Cr-10Fe-2Al-Ti-Y-Zr Seamless Tube 63Ni-25Cr-10Fe-2Al-Ti-Y-Zr Rod, Bar, & WireRod, Bar, 60Ni-23Cr-12Fe-Al ] Sheet, & Strip Plate, C 99.0Ni-Low 69] Pipe, Seamless 105] Plate, Sheet, 240] & Wire Rod, Bar, 72Ni-15Cr-8Fe 195] Plate, Sheet, & Strip 67Ni-30Cu 205] Seamless Tube 60Ni-23Cr-12Fe-Al 380/83] Pi Seamless 485/170]485/170]485/170] & Wire Rod, Bar, & Wire Rod, Bar, Seamless Pipe & Tube 67Ni-30Cu 67Ni-30Cu 67Ni-30Cu [345/69] & Bar Rod C 99.0Ni-Low [550/240][585/240] Seamless Tube Seamless Tube 72Ni-15Cr-8Fe 58Ni-29Cr-9Fe .5 [450/225] Castings 67Ni-30Cu-2Fe-Cb 10 [345/69] Fittings C 99.0Ni-Low 15 [380/105] Seamless Tube28 [485/195] 99.0Ni Seamless Tube25 [450/170]30 [450/205] 67Ni-30Cu Castings Castings 67Ni-30Cu-2Fe-Cb 67Ni-30Cu-Fe-Si Minimum Minimum Tensile/Yield Tensile/Yield 55/15 [380/105] Rod & Bar 99.0Ni 55/15 [380/105]55/15 [380/105] Fittings Forgings70/25 [485/170] 99.0Ni 99.0Ni Fittings70/25 [485/170] Forgings 67Ni-30Cu 67Ni-30Cu Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 4141 4141 41 ASTM/ASME 41 ASTM/ASME B/SB-160 ASTM/ASME B/SB-160 B/SB-161 — — — N02200 N02201 N02200 50/10 55/12 [ 41 41 ASTM/ASME B/SB-161 — N02201 50/10 [345/ 41 41 ASTM/ASME B/SB-162 — N02200 55/15 [380/ 4343 43 43 ASTM/ASME ASTM/ASME B/SB-166 B/SB-166 — — N06600 N06601 80/35 [550/ 80/30 [550/205] 4141 4141 4141 ASTM/ASME 4141 ASTM/ASME B/SB-162 4141 ASTM/ASME B/SB-163 4141 ASTM/ASME B/SB-163 4142 — ASTM/ASME B/SB-366 4142 — ASTM/ASME B/SB-366 4242 — B/SB-564 42 N0220142 — ASTM/ASME ASTM 42 N0220042 — ASTM/ASME B/SB-127 42 N0220142 — ASTM/ASME B/SB-163 42 N02200 42 B725 ASTM/ASME B/SB-164 42 N0220142 — ASTM/ASME B/SB-164 42 N02200 42 — ASTM/ASME B/SB-165 4242 — ASTM/ASME B/SB-366 — 50/12 [345/83 42 N0440043 — ASTM/ASME A/SA-494 55/ 42 N0440043 — ASTM/ASME A/SA-494 50/12 [345/83] 43 N0440043 — ASTM/ASME N02200 A/SA-494 M30C 43 N0440543 ASTM/ASME B/SB-564 M35-1 50/ 43 N0440043 ASTM/ASME B/SB-163 Seamless Tube M35-2 N24130 43 N04400 ASTM/ASME B/SB-163 N24135 43 — ASTM/ASME B/SB-163 N04020 70/28 [485/ — ASTM/ASME B/SB-163 70/ — B/SB-166 C 99.0Ni-Low 70/25 [ N04400 — 55/12 [380/83] 70/25 [ N06025 — 70/25 [ N06600 — 65/32 N06601 Pipe Welded 65/ N06690 65/ N06025 98/39 [675/270] 99.0Ni 80/35 80/30 [550/ 85/35 98/39 [675/270] Rod, Material Number
174 AWS B2.1/B2.1M-BMG:2014 p 60Ni-23Cr-12Fe-Al Strip 72Ni-15Cr-8Fe Strip 58Ni-29Cr-9Fe t Form Nominal Composition Fittings 62Ni-25Cr-9Fe-3Al-Cu-Ti-Zr Sheet, & Strip 63Ni-25Cr-10Fe-2Al-Ti-Y-Zr less Pipe & Tube 63Ni-25Cr-10Fe-2Al-Ti-Y-Zr e, Sheet, & Strip 53Ni-22Cr-14W-Co-Fe-Mo ate, Sheet, & Stri ate, Sheet, & Strip 52Ni-22Cr-13Co-9Mo ate, Sheet, & Stripate, Sheet, & Strip 47Ni-22Cr-9Mo-18Fe ate, Sheet, & Strip 60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb amless Pipe & Tube 60Ni-23Cr-12Fe-Al Rod, Bar, & WireRod, Bar, 52Ni-22Cr-13Co-9Mo Plate, Sheet, & Plate, Sheet, & Seamless Pipe & Tube 52Ni-22Cr-13Co-9Mo 310] Fittings 53Ni-22Cr-14W-Co-Fe-Mo 240]170] & Wire Rod, Bar, Seamless Pipe & Tube 58Ni-29Cr-9Fe 72Ni-15Cr-8Fe 175] Seamless Pipe & Tube 58Ni-29Cr-9Fe 270] Fittings 63Ni-25Cr-10Fe-2Al-Ti-Y-Zr 760/380] Fittings 60Ni-22Cr-9Mo-3.5Cb 690/275]690/310] Fittings Fittings690/310]690/310] 47Ni-22Cr-18Fe-9Mo Fittings 55Ni-21Cr-13.5Mo Fittings 59Ni-23Cr-16Mo-1.6Cu 60Ni-19Cr-19Mo-1.8Ta [690/285] Fittings 54Ni-16Mo-15Cr [690/310] Fittings[690/275] Fittings 59Ni-23Cr-16Mo 61Ni-15Mo-16Cr 35 [585/240] Fittings35 [550/240] 58Ni-33Cr-8Mo Fittings 72Ni-15Cr-8Fe Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 43 46 ASTM/ASME B/SB-166 — N06617 95/35 [655/240] 4343 4343 4343 ASTM/ASME 4343 ASTM/ASME B/SB-166 43 ASTM/ASME B/SB-167 46 ASTM/ASME B/SB-16743 — ASTM/ASME B/SB-167 — B/SB-167 43 — N06690 — ASTM/ASME N06025 — B/SB-168 N06600 N06601 N06617 — 85/35 [585/ N06600 98/39 [675/270] 75/25 [515/ Seam 80/30 [550/205] 95/35 [655/240] Se 80/35 [550/240] 4343 43 4343 ASTM/ASME ASTM/ASME B/SB-167 43 B/SB-168 ASTM/ASME — B/SB-168 — N06690 — N06025 N06601 75/25 [515/ 98/39 [675/270] Plate, 80/30 [550/205] Pl 4343 46 43 ASTM/ASME ASTM/ASME B/SB-168 B/SB-168 — — N06617 N0669043 95/35 [655/240]43 85/35 [585/240] 4343 Pl 43 ASTM/ASME 43 ASTM/ASME B/SB-435 ASTM/ASME B/SB-443 B/SB-443 — 1 2 N06230 N06625 N06625 110/45 [760/310] 110/55 [760/380] Plat 100/40 [690/275] Pl Pl 4343 4343 43 ASTM/ASME 43 ASTM/ASME B/SB-366 ASTM/ASME B/SB-366 B/SB-435 — — — N06625 N10276 N06002 110/55 [ 100/41 95/35 [655/240] Pl 4343 4343 4443 ASTM/ASME 4343 ASTM/ASME B/SB-366 4343 ASTM/ASME B/SB-366 4343 ASTM/ASME B/SB-366 4343 — ASTM/ASME B/SB-366 4343 — ASTM/ASME B/SB-366 4343 — ASTM/ASME B/SB-366 43 N0600243 — ASTM/ASME B/SB-366 43 N06022 — ASTM/ASME B/SB-366 43 N06025 — ASTM/ASME B/SB-366 N06035 — ASTM/ASME B/SB-366 N06059 — B/SB-366 N06200 — N06210 — 100/40 [ N06230 — 100/45 [ N06455 98/39 [675/ N06600 85/ N06603 100/45 100/45 [ 100/45 [ 110/45 [760/ 100/40 80/ 94/43 [650/295] Material Number
175 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition lded Pipe 62Ni-25Cr-9Fe-3Al-Cu-Ti-Zr lded Tube 62Ni-25Cr-9Fe-3Al-Cu-Ti-Zr Welded TubeWelded 63Ni-25Cr-10Fe-2Al-Ti-Y-Zr Seamless Pipe & TubeSeamless Pipe & Tube 60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb 415]275] Rod & Bar Rod & Bar310] 60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb Forgings 58Ni-21Cr-16Mo-3.5N 690/310]690/310] Forgings Forgings 55Ni-21Cr-13.5Mo 59Ni-23Cr-16Mo-1.6Cu 690/310] Forgings 55Ni-21Cr-13.5Mo [690/310] Forgings 59Ni-23Cr-16Mo [690/310][690/285] Forgings Forgings 59Ni-23Cr-16Mo 54Ni-16Mo-15Cr [485/275][550/310] Castings Castings 60Ni-21.5Cr-9Mo-4Cb-Fe 59Ni-22Cr-14Mo-4Fe-3W 35 [585/240] Forgings 58Ni-33Cr-8Mo 35 [585/240] Forgings40 [495/275]28 [485/195] 58Ni-33Cr-8Mo Castings Castings 66Ni-16Mo-16Cr-Fe-W 72Ni-15Cr-8Fe-Si Minimum Minimum Tensile/Yield Tensile/Yield 90/40 [620/275] Forgings 51Ni-30Cr-10Mo-W 84/39 [580/270] Forgings 63Ni-25Cr-10Fe-2Al-Ti-Y-Zr Strength, ksi [MPa] Produc 254] 305] 10 12 ≤ ≤ ≤ ≤ 102] 95/45 [655/310] Forgings 51Ni-30Cr-10Mo-W 100] 98/39 [675/270] Forgings 63Ni-25Cr-10Fe-2Al-Ti-Y-Zr ≤ ≤ [mm] 4 [ 4 [ Diameter Diameter ≤ ≤ .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, [>102 and [>102 and [>100 and [>100 and Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 43 43 ASTM/ASME B/SB-564 — N06110 4343 4343 43 ASTM/ASME 43 ASTM/ASME B/SB-564 ASTM/ASME B/SB-564 B/SB-564 — — — N06035 N06059 N06110 and >4 85/ 100/45 4343 4343 4343 ASTM/ASME 4343 ASTM/ASME B/SB-444 4443 ASTM/ASME B/SB-446 4343 ASTM/ASME B/SB-446 4343 ASTM/ASME 2 B/SB-462 4343 ASTM/ASME 1 B/SB-462 4343 ASTM/ASME 2 B/SB-462 4343 — ASTM/ASME N06625 B/SB-462 4343 — ASTM/ASME N06625 B/SB-462 4343 — ASTM/ASME N06625 B/SB-462 44 N0602243 — ASTM/ASME A/SA-494 43 N06035 — ASTM/ASME A/SA-494 43 N06059 — ASTM/ASME A/SA-494 CW2M N06200 CW6MC ASTM/ASME A/SA-494 100/40 [690/275] N06686 CX2MW B/SB-516 N26455 120/60 [825/ N10276 N26625 CY40 100/40 [690/ N2602243 100/45 [ 43 — 85/ N06040 4443 100/45 43 ASTM/ASME 100/45 [ 43 N06025 ASTM/ASME B/SB-564 100/45 [690/ ASTM/ASME 72/ B/SB-564 100/41 70/40 B/SB-564 80/45 — — 70/ — N06022 98/39 [675/270] N06025 N06025 and >4 100/45 [ 43 43 ASTM/ASME B/SB-444 1 N06625 120/60 [825/415] 4343 4343 4343 ASTM/ASME 4343 ASTM/ASME B/SB-516 43 ASTM/ASME B/SB-516 43 ASTM/ASME B/SB-517 — ASTM/ASME B/SB-517 — B/SB-517 — N06600 — N06603 — N06025 N06600 N06603 80/35 [550/240] 94/43 [650/295] 98/39 [675/270] Tube Welded 80/35 [550/240] We 94/43 [650/295] Pipe Welded Pipe Welded We 72Ni-15Cr-8Fe 63Ni-25Cr-10Fe-2Al-Ti-Y-Zr 72Ni-15Cr-8Fe Material Number
176 AWS B2.1/B2.1M-BMG:2014 Strip 58Ni-33Cr-8Mo Strip 61Ni-16Mo-16Cr t Form Nominal Composition Forgings 62Ni-25Cr-9Fe-3Al-Cu-Ti-Zr ate, Sheet, & Strip 55Ni-21Cr-13.5Mo ate, Sheet, & Stripate, Sheet, & Strip 59Ni-23Cr-16Mo-1.6Cu 60Ni-19Cr-19Mo-1.8Ta ate, Sheet, & Strip 58Ni-21Cr-16Mo-3.5W Plate, Sheet, & Plate, Sheet, & Strip 59Ni-23Cr-16Mo Plate, Sheet, & 310] Forgings 53Ni-22Cr-14W-Co-Fe-Mo 690/310]690/310] Forgings Forgings 59Ni-23Cr-16Mo-1.6Cu 60Ni-19Cr-19Mo-1.8Ta 690/310] Forgings760/310] 58Ni-21Cr-16Mo-3.5W Rod 53Ni-22Cr-14W-Co-Fe-Mo [690/285][690/310] Forgings[690/310] Rod 54Ni-16Mo-15Cr [690/310] Rod 55Ni-21Cr-13.5Mo Rod 59Ni-23Cr-16Mo-1.6Cu 58Ni-21Cr-16Mo-3.5W [655/240] Forgings 52Ni-22Cr-13Co-9Mo 35 [550/240] Forgings35 [585/240] 72Ni-15Cr-8Fe 35 [655/240] Forgings Rod 58Ni-29Cr-9Fe 47Ni-22Cr-9Mo-18Fe Minimum Minimum Tensile/Yield Tensile/Yield 110/50 [760/345] Forgings 60Ni-22Cr-9Mo-3.5Cb Strength, ksi [MPa] Produc 254] 10 ≤ ≤ 102] 120/60 [825/415] Forgings 60Ni-22Cr-9Mo-3.5Cb ≤ [mm] 4 [ Diameter Diameter ≤ .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, [>102 and [>102 and Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 43 43 ASTM/ASME B/SB-564 — N06200 100/45 [ 4343 4343 4343 ASTM/ASME 43 ASTM/ASME B/SB-564 43 ASTM/ASME B/SB-564 ASTM/ASME B/SB-56443 — B/SB-56443 — 4343 — 4343 N06210 ASTM/ASME — 4343 N06230 ASTM/ASME B/SB-564 4343 N06600 ASTM/ASME B/SB-564 4343 N06603 ASTM/ASME B/SB-564 4343 — ASTM/ASME B/SB-564 4443 — ASTM/ASME B/SB-572 4343 — ASTM/ASME B/SB-572 100/45 [ 43 N06625 43 — ASTM/ASME B/SB-574 110/45 [760/ 43 N0668643 — ASTM/ASME B/SB-574 43 N06690 80/ 43 — ASTM/ASME B/SB-574 43 N10276 94/43 [650/295] 43 — ASTM/ASME B/SB-574 43 N0600243 — ASTM/ASME B/SB-574 43 N06230 — ASTM/ASME B/SB-574 44 N06022 — ASTM/ASME B/SB-574 N06035 — ASTM/ASME B/SB-574 100/45 [ N06059 — B/SB-575 85/ N06200 — 100/41 N06210 — 95/ N06455 — 110/45 [ N06686 100/45 N10276 85/35 [585/240] N06022 100/45 [690/310] 100/45 100/45 [690/310] 100/40 [690/275] Rod Rod 100/45 100/41 [690/285] Rod 100/45 [690/310] Rod Pl 58Ni-33Cr-8Mo Rod 59Ni-23Cr-16Mo 60Ni-19Cr-19Mo-1.8Ta 61Ni-16Mo-16Cr 54Ni-16Mo-15Cr 4343 46 43 ASTM/ASME ASTM/ASME B/SB-564 B/SB-564 — — N06617 N06625 and >4 95/35 43 4343 ASTM/ASME43 B/SB-575 43 43 ASTM/ASME — ASTM/ASME B/SB-575 B/SB-575 N06035 — — N06210 N06455 85/35 [585/240] 100/45 [690/310] 100/40 [690/275] Pl 43 43 ASTM/ASME B/SB-575 — N06200 100/45 [690/310] Pl 43 43 ASTM/ASME43 B/SB-575 43 — ASTM/ASME B/SB-575 N06059 — N06686 100/45 [690/310] 100/45 [690/310] Pl Material Number
177 AWS B2.1/B2.1M-BMG:2014 57Ni-21Cr-13Mo-6Fe-Cu-(Cb+Ta) Strip 54Ni-16Mo-15Cr t Form Nominal Composition amless Pipe & Tubeamless Pipe & Tube 53Ni-22Cr-14W-Co-Fe-Mo 52Ni-21Cr-13Fe-11Mo-W-Cu amless Pipe & Tube 50Ni-24Cr-17Fe-7Mo-W Plate, Sheet, & Seamless Pipe & TubeSeamless Pipe & Tube 59Ni-23Cr-16Mo-1.6Cu 60Ni-19Cr-19Mo-1.8Ta Seamless Pipe & TubeSeamless Pipe & Tube 47Ni-22Cr-9Mo-18Fe 55Ni-21Cr-13.5Mo Seamless Pipe & Tube 58Ni-21Cr-16Mo-3.5W 5] Seamless Pipe & Tube 61Ni-16Mo-16Cr 0] Pipe Welded 53Ni-22Cr-14W-Co-Fe-Mo 0] Seamless Pipe & Tube 59Ni-23Cr-16Mo 5] Seamless Pipe & Tube 54Ni-16Mo-15Cr 275]310] Pipe Welded Pipe Welded 310] 47Ni-22Cr-9Mo-18Fe Pipe Welded 55Ni-21Cr-13.5Mo 310] 59Ni-23Cr-16Mo-1.6Cu Pipe Welded 58Ni-21Cr-16Mo-3.5W 275]310] Tube Welded Tube Welded 310] 47Ni-22Cr-9Mo-18Fe Tube Welded 55Ni-21Cr-13.5Mo 59Ni-23Cr-16Mo-1.6Cu 240] Seamless Pipe & Tube 58Ni-33Cr-8Mo 35 [620/240] Seamless Pipe & Tube Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 4343 43 43 ASTM/ASME ASTM/ASME B/SB-622 B/SB-622 — — N06210 N06230 100/45 [690/310] 110/45 [760/310] Se 43 43 ASTM/ASME B/SB-575 — N1027643 100/41 [690/285] 43 ASTM/ASME B/SB-622 — N06200 100/45 [690/310] 4343 4343 4343 ASTM/ASME 43 ASTM/ASME B/SB-622 43 ASTM/ASME B/SB-622 ASTM/ASME B/SB-622 — B/SB-622 — — N06250 — N06255 N06455 N06686 90/35 [620/240] 85/32 [585/220] Se 100/40 [690/27 Se 100/45 [690/310] 4343 4343 4443 ASTM/ASME 4343 ASTM/ASME B/SB-619 4343 ASTM/ASME B/SB-619 4343 ASTM/ASME B/SB-619 4343 — ASTM/ASME B/SB-619 4343 — ASTM/ASME B/SB-619 4343 — ASTM/ASME B/SB-619 43 N0600243 — ASTM/ASME B/SB-619 43 N0602243 — ASTM/ASME B/SB-619 43 N0603543 — ASTM/ASME B/SB-619 44 N0605943 — ASTM/ASME B/SB-619 43 N0620043 — ASTM/ASME B/SB-622 43 N06210 — ASTM/ASME B/SB-622 43 N06230 — ASTM/ASME B/SB-622 100/40 [690/ N06455 — ASTM/ASME B/SB-622 100/45 [690/ N06686 — B/SB-622 85/35 [585/240] N10276 — 100/45 [690/310] N06002 — 100/45 [690/ N06022 — Pipe Welded 100/45 [690/310] N0603543 Pipe Welded 110/45 [760/31 N0605943 100/40 [690/275] 43 N0606043 Pipe Welded 100/45 [690/ 4343 ASTM/ASME 100/41 [690/285] 58Ni-33Cr-8Mo 4443 Pipe Welded 59Ni-23Cr-16Mo ASTM/ASME B/SB-622 100/40 [690/275] 4343 ASTM/ASME 60Ni-19Cr-19Mo-1.8Ta B/SB-626 100/45 [690/310] 43 Pipe Welded ASTM/ASME B/SB-626 85/35 [585/ 43 — ASTM/ASME B/SB-626 100/45 [690/31 61Ni-16Mo-16Cr — ASTM/ASME B/SB-626 90/ — B/SB-626 N10276 54Ni-16Mo-15Cr — N06002 — N06022 — N06035 N06059 N06200 100/41 [690/28 100/40 [690/ 100/45 [690/ 85/35 [585/240] 100/45 [690/310] 100/45 [690/ Tube Welded Tube Welded 58Ni-33Cr-8Mo 59Ni-23Cr-16Mo Material Number
178 AWS B2.1/B2.1M-BMG:2014 p 60Ni-23Mo-8Cr-6.5Fe p 65Ni-29.5Mo-2Fe-2Cr Strip 65Ni-28Mo-2Fe & Strip 62Ni-28Mo-5Fe t, & Strip 62Ni-28Mo-5Fe t Form Nominal Composition Sheet, & Strip 66Ni-28Mo-3Fe-1.3Cr-0.25Al ate, Sheet, & Stri ate, Sheet, & Stri Plate, Sheet, & 0] Tube Welded 53Ni-22Cr-14W-Co-Fe-Mo 310] Tube Welded 58Ni-21Cr-16Mo-3.5W 350] Rod 66Ni-28Mo-3Fe-1.3Cr-0.25Al 795/345] Plate, Sheet, [715/315] Rod 60Ni-23Mo-8Cr-6.5Fe Minimum Minimum Tensile/Yield Tensile/Yield 90/40 [620/275] Rod & Bar 51Ni-30Cr-10Mo-W 100/45 [690/310] Plate, Shee 115/46 [795/315] Rod 62Ni-28Mo-5Fe 100/46 [690/315] Rod 62Ni-28Mo-5Fe Strength, ksi [MPa] Produc 2.5 1.5 ≤ ≤ 64] 254] 3.5 89] 10 38] ≤ ≤ ≤ ≤ ≤ ≤ 102] 95/45 [655/310] Rod & Bar 51Ni-30Cr-10Mo-W ≤ [mm] 4 [ 8 and Diameter Diameter ≤ 4.8 and ≥ .2 (Continued) Thickness or [ ≥ [>38 and [>38 and (Continued) Limitations, in in Limitations, 0.1875 and 0.3125 and [ [>102 and [>102 and ≥ ≥ Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 44 44 ASTM/ASME B/SB-333 — N10624 104/46 [715/315] Pl 4343 4343 4343 4344 ASTM 4344 ASTM 44 ASTM 44 B756 ASTM/ASME ASTM B757 ASTM/ASME B/SB-333 B758 B/SB-333 B759 — — — — — N06110 — N10001 N06110 N10001 N06110 [<48] <0.1875 N06110[ 115/50 95/45 [655/310] 95/45 [655/310] 95/45 [655/310] Pipe Welded Seamless Pipe & Tube Tube Welded 51Ni-30Cr-10Mo-W 51Ni-30Cr-10Mo-W 51Ni-30Cr-10Mo-W 4343 4343 4343 ASTM/ASME 4343 ASTM/ASME B/SB-626 4343 ASTM/ASME B/SB-626 4343 ASTM/ASME B/SB-626 43 — ASTM/ASME B/SB-704 43 — B/SB-705 — ASTM N06455 — ASTM N06686 — N10276 B755 N06625 B756 N06625 — 100/40 [690/275] — 100/45 [690/ N06110 100/41 [690/285] Tube Welded N06110 120/60 [825/415] 120/60 [825/415] Tube Welded and >4 Tube Welded 61Ni-16Mo-16Cr Pipe Welded 54Ni-16Mo-15Cr 95/45 [655/310] 60Ni-22Cr-9Mo-3.5Cb 60Ni-22Cr-9Mo-3.5Cb Plate, Sheet, & Strip 51Ni-30Cr-10Mo-W 4343 43 43 ASTM/ASME ASTM/ASME B/SB-626 B/SB-626 — — N06210 N06230 100/45 [690/310] 110/45 [760/31 Tube Welded 60Ni-19Cr-19Mo-1.8Ta 44 44 ASTM/ASME B/SB-333 — N10665 110/51 [760/350] 44 4444 ASTM/ASME 44 B/SB-333 ASTM/ASME B/SB-33344 —44 4444 — 4444 ASTM/ASME N10629 44 ASTM/ASME B/SB-335 44 ASTM/ASME N10675 B/SB-335 ASTM/ASME B/SB-335 — B/SB-335 — — N10624 110/51 [760/350] — N10629 Plate, N10665 110/51 [760/350] N10675 Pl 104/46 110/51 [760/ 110/51 [760/350] 110/51 [760/350] Rod Rod 65Ni-28Mo-2Fe 65Ni-29.5Mo-2Fe-2Cr 4444 44 ASTM/ASME 44 B/SB-335 ASTM/ASME B/SB-335 — — N10001 and >1.5 N10001 Material Number
179 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition Welded PipeWelded 66Ni-28Mo-3Fe-1.3Cr-0.25Al ate, Sheet, & Stripate, Sheet, & Strip 70Ni-16Mo-7Cr-5Fe 62Ni-25Mo-8Cr-2Fe Seamless Pipe & Tube 62Ni-25Mo-8Cr-2Fe 0] Seamless Pipe & Tube 62Ni-28Mo-5Fe 0] Fittings0] 66Ni-28Mo-3Fe-1.3Cr-0.25Al Forgings 66Ni-28Mo-3Fe-1.3Cr-0.25Al 0] Forgings 66Ni-28Mo-3Fe-1.3Cr-0.25Al 310]315] Pipe Welded Pipe Welded 62Ni-25Mo-8Cr-2Fe 60Ni-23Mo-8Cr-6.5Fe 690/275]725/310]715/315] Fittings Fittings760/350] Fittings 70Ni-16Mo-7Cr-5Fe Fittings 62Ni-25Mo-8Cr-2Fe 60Ni-23Mo-8Cr-6.5Fe 760/350] 65Ni-29.5Mo-2Fe-2Cr 725/310] Forgings715/315] Forgings 65Ni-29.5Mo-2Fe-2Cr 760/350] Forgings Forgings 62Ni-25Mo-8Cr-2Fe 60Ni-23Mo-8Cr-6.5Fe 65Ni-29.5Mo-2Fe-2Cr 525/275] Castings 65Ni-31.5Mo-1.5Fe-Cr [690/310] Fittings[760/350] 62Ni-28Mo-5Fe Fittings[760/350] Forgings 65Ni-28Mo-2Fe [760/350] 65Ni-28Mo-2Fe [690/275][725/310] Forgings Rod Rod 65Ni-28Mo-2Fe 70Ni-16Mo-7Cr-5Fe 62Ni-25Mo-8Cr-2Fe 40 [495/275] Castings 56Ni-19Mo-18Cr-2Fe Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 4444 4444 4444 ASTM/ASME 44 ASTM/ASME B/SB-619 44 ASTM/ASME B/SB-619 ASTM/ASME B/SB-622 — B/SB-622 — — N10665 — N10675 N10001 N10242 110/51 [760/350] 110/51 [760/350] 100/45 [690/31 Pipe Welded 105/45 [725/310] Pipe Welded 65Ni-28Mo-2Fe 65Ni-29.5Mo-2Fe-2Cr 4444 4444 4444 ASTM/ASME 4444 ASTM/ASME B/SB-366 4444 ASTM/ASME B/SB-366 4444 ASTM/ASME B/SB-366 4444 — ASTM/ASME B/SB-366 4444 — ASTM/ASME B/SB-366 4444 — ASTM/ASME B/SB-366 44 N1000344 — ASTM/ASME B/SB-434 44 N1024244 — ASTM/ASME B/SB-434 44 N1062444 — ASTM/ASME B/SB-462 44 N1062944 — ASTM/ASME B/SB-462 44 N1066544 — ASTM/ASME B/SB-462 44 N1067544 — ASTM/ASME A/SA-494 44 N1000344 — ASTM/ASME A/SA-494 100/40 [ 44 N1024244 — ASTM/ASME CW6M B/SB-564 105/45 [ 44 N1062944 ASTM/ASME B/SB-564 104/46 [ N7M 44 N1066544 ASTM/ASME B/SB-564 N30107 110/51 [760/35 44 N1067544 — ASTM/ASME B/SB-564 110/51 4444 N30007 — ASTM/ASME B/SB-564 110/51 [ 4444 — ASTM/ASME B/SB-573 100/40 [690/275] 44 N1024244 — ASTM/ASME B/SB-573 105/45 [725/310] 44 N10624 Pl — ASTM/ASME B/SB-619 110/51 [760/35 44 N10629 Pl — ASTM/ASME B/SB-619 110/51 N10665 — ASTM/ASME 72/ B/SB-619 110/51 [ N10675 — B/SB-619 76/40 [ N10003 — N10242 — 105/45 [ N10001 — 104/46 [ N10242 110/51 [760/35 N10624 110/51 N10629 110/51 [ 100/40 105/45 100/45 [690/310] 105/45 [725/ 104/46 [715/ Pipe Welded 110/51 [760/350] 62Ni-28Mo-5Fe 44 44 ASTM/ASME B/SB-366 — N10001 100/45 Material Number
180 AWS B2.1/B2.1M-BMG:2014 1W-Mn-Si-Al Pipe 46Fe-24Ni-21Cr-6Mo-Cu-N t Form Nominal Composition less Pipe & Tube 66Ni-28Mo-3Fe-1.3Cr-0.25Al e, Sheet, & Strip 44Fe-25Ni-21Cr-Mo Welded TubeWelded 66Ni-28Mo-3Fe-1.3Cr-0.25Al less & Welded Pipeless & Welded Pipeless & Welded 46Fe-24Ni-21Cr-6Mo-Cu-N 44Fe-25Ni-21Cr-Mo Seamless Tube 42Ni-21.5Cr-3Mo-2.3Cu Seamless Pipe & Tube 65Ni-29.5Mo-2Fe-2Cr Seamless Pipe & Tube 60Ni-23Mo-8Cr-7Fe 0] Seamless Pipe & Tube 65Ni-28Mo-2Fe 310]315] Tube Welded Tube Welded 62Ni-25Mo-8Cr-2Fe 60Ni-23Mo-8Cr-6.5Fe 170] Seamless Tube 33Ni-42Fe-21Cr-Al-Ti 450/170] Seamless Tube 32Ni-45Fe-20.5Cr-Ti [620/275][515/205] Seamless Tube[450/170] Seamless Tube Seamless Tube 37Ni-33Fe-25Cr 33Ni-42Fe-21Cr 33Ni-42Fe-21Cr Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc 5] 100/45 [690/310] Seamless & Welded 5] 100/45 [690/310] Tube Welded 46Fe-24Ni-21Cr-6Mo-Cu-N 5] 95/45 [655/310] Plate 46Fe-24Ni-21Cr-6Mo-Cu-N ≤ ≤ ≥ [mm] Diameter Diameter 0.1875 [ 0.1875 [ 0.1875 [ .2 (Continued) Thickness or ≤ ≤ ≥ (Continued) Limitations, in in Limitations, Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 45 8.2 ASTM/ASME A/SA-351 CN7M N08007 62/25 [425/170] Castings 28Ni-19Cr-Cu-Mo 4545 8.245 8.245 8.245 ASTM/ASME ASTM 8.2 A/SA-249 8.2 ASTM A249 ASTM — ASTM A312 A312 — N08904 A312 — N08367 N08367 N08367 N08367 [>5] >0.1875 N08904 N08367 [>5] >0.1875 95/45 [655/310] 71/31 [490/215] 95/45 [655/310] Seam Tube Welded Tube Welded 46Fe-24Ni-21Cr-6Mo-Cu-N 71/31 [490/215] Seam 44Fe-25Ni-21Cr-Mo 4545 8.2 8.2 ASTM ASTM A240 A249 904L — N08904 N08367 71/31 [490/215] Plat 4444 4444 44 ASTM/ASME 43 ASTM/ASME B/SB-626 B/SB-626 AMS — — 5711 N10665 N10675 — N06635 110/51 [760/350] 110/51 [760/350] Tube Welded Tube Welded 185/120 [1275/825] 65Ni-28Mo-2Fe 65Ni-29.5Mo-2Fe-2Cr Sheet 62Ni-16Cr-15Mo-3Fe-2Co- 4444 4444 4444 ASTM/ASME 44 ASTM/ASME B/SB-626 44 ASTM/ASME B/SB-626 ASTM/ASME B/SB-626 — B/SB-62645 —45 — 4545 N10001 — 4545 N10242 ASTM/ASME 4545 N10624 ASTM/ASME B/SB-163 4545 N10629 ASTM/ASME B/SB-163 4545 ASTM/ASME B/SB-163 4545 — ASTM/ASME B/SB-163 8.245 — ASTM/ASME B/SB-163 100/45 [690/310] 8.2 — B/SB-163 105/45 [725/ 8.2 N08120 ASTM — 104/46 [715/ N08800 ASTM — Tube Welded 110/51 [760/350] N08801 ASTM — N08810 A182 N08811 A240 N08825 A240 62Ni-28Mo-5Fe F904L 90/40 — 75/30 N08904 — 65/25 [ 65/25 N08367 65/25 [450/ N08367 85/35 [585/240] [<5] <0.1875 100/45 [690/310] 71/31 [490/215] Sheet & Strip 46Fe-24Ni-21Cr-6Mo-Cu-N Forgings 44Fe-25Ni-21Cr-Mo 4444 44 44 ASTM/ASME ASTM/ASME B/SB-622 B/SB-622 — — N10665 N10675 110/51 [760/35 110/51 [760/350] 44 44 ASTM/ASME B/SB-622 — N10629 110/51 [760/350] Seam 44 44 ASTM/ASME B/SB-622 — N10624 104/46 [715/315] Material Number
181 AWS B2.1/B2.1M-BMG:2014 3W 0.6Cu-N t Form Nominal Composition amless Pipe & Tube 33Ni-42Fe-21Cr-Al-Ti Fusion Welded PipeFusion Welded 46Fe-24Ni-21Cr-6Mo-Cu-N Seamless Pipe & Tube 32Ni-45Fe-20.5Cr-Ti 310] Fittings 21Ni-30Fe-22Cr-18Co-3Mo- 240] Fittings 42Ni-21.5Cr-3Mo-2.3Cu 275]205] Seamless Pipe & Tube Seamless Pipe & Tube170] 37Ni-33Fe-25Cr Seamless Pipe & Tube 33Ni-42Fe-21Cr 33Ni-42Fe-21Cr 750/380] Fittings 33Cr-31Ni-32Fe-1.5Mo- 450/170] Fittings 33Ni-42Fe-21Cr-Al-Ti [620/240][585/240][620/240][550/240] Fittings[650/275] Fittings Fittings Fittings Fittings 47Ni-22Cr-19Fe-6Mo 40Ni-29Cr-15Fe-5Mo 47Ni-22Cr-20Fe-7Mo 35Ni-35Fe-20Cr-Cb 31Ni-31Fe-27Cr-7Mo [620/275][515/205] Rod & Bar Rod & Bar 37Ni-33Fe-25Cr 33Ni-42Fe-21Cr 45 [655/310]30 [515/205]25 [450/170] Fittings Fittings31 [490/215] Fittings 46Fe-24Ni-21Cr-6Mo-Cu-N Fittings 33Ni-42Fe-21Cr 33Ni-42Fe-21Cr 44Fe-25Ni-21Cr-Mo 40 [620/275] Fittings 37Ni-33Fe-25Cr 25 [435/170] Castings 32Ni-45Fe-20Cr-Cb Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc 5] 100/45 [690/310] Pipe Fusion Welded 46Fe-24Ni-21Cr-6Mo-Cu-N 4.8] 100/45 [690/310] Fittings 46Fe-24Ni-21Cr-6Mo-Cu-N ≤ ≤ [mm] Diameter Diameter 0.1875 [ .2 (Continued) 0.1875 [ Thickness or ≤ (Continued) Limitations, in in Limitations, ≤ Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 4545 8.245 4545 ASTM/ASME 4545 ASTM/ASME B/SB-366 4545 ASTM/ASME B/SB-366 4545 ASTM/ASME B/SB-366 8.245 — ASTM/ASME B/SB-366 8.245 ASTM/ASME — B/SB-366 8.2 ASTM/ASME — B/SB-366 N08367 45 ASTM/ASME — B/SB-366 N08800 >0.1875 [>4.8] — ASTM/ASME B/SB-366 N08810 — 95/ B/SB-366 N08811 — N08825 — N08904 — N08925 N08926 75/ R20033 65/ 65/25 [ 85/35 [585/ 71/ 87/43 [600/295] 94/43 [650/295] 109/55 [ Fittings Fittings 25Ni-20Cr-6Mo-Cu-N 25Ni-20Cr-6Mo-Cu-N 45 45 ASTM/ASME B/SB-366 — R30556 100/45 [690/ 45 8.2 ASTM A358 N08367 N08367 [>5] >0.1875 95/45 [655/310] 4545 4345 4545 ASTM/ASME 4545 ASTM/ASME B/SB-366 4545 ASTM/ASME B/SB-366 4545 ASTM/ASME B/SB-366 45 — ASTM/ASME B/SB-366 8.2 — ASTM/ASME B/SB-366 ASTM/ASME — B/SB-366 N06007 — B/SB-366 N06030 — N06985 — N08020 — N08031 N08120 N08367 90/35 85/35 90/35 80/35 94/40 90/ 4545 4545 4545 ASTM/ASME 4545 ASTM/ASME B/SB-407 45 ASTM/ASME B/SB-407 45 ASTM/ASME B/SB-407 — ASTM/ASME B/SB-407 — B/SB-407 — N08120 — N08800 — N08801 N08810 N08811 90/40 [620/ 75/30 [515/ 65/25 [450/170] 65/25 [450/ 65/25 [450/170] Se 4545 45 45 ASTM/ASME ASTM/ASME B/SB-408 B/SB-408 — — N08120 N08800 90/40 75/30 45 45 ASTM/ASME A/SA-351 CT15C N08151 63/ 45 8.2 ASTM A358 N08367 N08367 Material Number
182 AWS B2.1/B2.1M-BMG:2014 3W 0.6Cu-N 2Ni-21.5Cr-3Mo-2.3Cu p 37Ni-33Fe-23Cr-4Mo t Form Nominal Composition Sheet, & Strip 35Ni-30Fe-24Cr-6Mo-3Cu less Pipe & Tube 42Ni-21.5Cr-3Mo-2.3Cu Welded PipeWelded 35Ni-30Fe-24Cr-6Mo-3Cu e, Sheet, & Strip 33Ni-42Fe-21Cr-Al-Ti e, Sheet, & Stripe, Sheet, & Strip 42Ni-21Cr-6Mo-2.3Cu 4 e, Sheet, & Strip 21Ni-30Fe-22Cr-18Co-3Mo- ate, Sheet, & Stripate, Sheet, & Stri 35Ni-35Fe-20Cr-Cb amless Pipe & Tube 42Ni-21Cr-6Mo-2.3Cu Plate, Sheet, & StripPlate, Sheet, & StripPlate, Sheet, & Strip 37Ni-33Fe-25Cr 33Ni-42Fe-21Cr 33Ni-42Fe-21Cr 240] Rod & Bar 42Ni-21.5Cr-3Mo-2.3Cu 240]275] Forgings Forgings 35Ni-30Fe-24Cr-6Mo-3Cu 31Ni-33Fe-22Cr-6.5Mo-Cu-N 750/380] Forgings 33Cr-31Ni-32Fe-1.5Mo- 450/170] Rod & Bar 33Ni-42Fe-21Cr-Al-Ti 545/235] Rod & Bar 42Ni-21Cr-6Mo-2.3Cu 550/240] Pipe Welded 550/240] Tube Welded 35Ni-35Fe-20Cr-Cb 35Ni-35Fe-20Cr-Cb [450/170] Rod & Bar 33Ni-42Fe-21Cr [585/240][550/240][550/240] Forgings Forgings Forgings 40Ni-29Cr-15Fe-5Mo 35Ni-35Fe-20Cr-Cb 37Ni-33Fe-23Cr-4Mo Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 45 45 ASTM/ASME B/SB-408 — N08810 65/25 4545 4545 4545 ASTM/ASME 4545 ASTM/ASME B/SB-408 45 ASTM/ASME B/SB-409 4545 ASTM/ASME B/SB-40945 — ASTM/ASME B/SB-409 45 — B/SB-409 45 — ASTM/ASME N08811 — ASTM/ASME B/SB-423 N08120 — B/SB-424 N08800 N08810 — N08811 — N08825 65/25 [ N08221 90/40 [620/275] 75/30 [515/205] 65/25 [450/170] 65/25 [450/170] Plat 75/25 [515/170] 79/34 [545/235] Seam Plat 45 4545 ASTM/ASME45 B/SB-423 4545 4545 ASTM/ASME 45 — ASTM/ASME B/SB-424 45 ASTM/ASME B/SB-425 ASTM/ASME B/SB-425 N08221 — B/SB-435 — — N08825 — N08221 N08825 R30556 79/34 [545/235] Se 85/35 [585/240] 79/34 [ Plat 85/35 [585/ 100/45 [690/310] Plat 4545 4545 4545 ASTM/ASME 4545 ASTM/ASME B/SB-462 4545 ASTM/ASME B/SB-462 4545 ASTM/ASME B/SB-462 8.2 — ASTM/ASME B/SB-46245 45 ASTM/ASME — B/SB-46245 — ASTM/ASME B/SB-462 45 N06030 — B/SB-462 45 N08020 ASTM/ASME — N08024 ASTM/ASME — B/SB-463 N08026 B/SB-463 — N08031 N08367 — R20033 — 85/35 N08020 80/35 N08024 80/35 80/35 [550/ 94/40 [650/ 95/45 [655/310] 109/55 [ 80/35 [550/240] Forgings 80/35 [550/240] Pl Pl 46Fe-24Ni-21Cr-6Mo-Cu-N 4545 4545 4545 ASTM/ASME 45 ASTM/ASME B/SB-464 45 ASTM/ASME B/SB-464 ASTM/ASME B/SB-464 — B/SB-468 — — N08020 — N08024 N08026 N08020 80/35 [ 80/35 [550/240] 80/35 [550/240] 80/35 [ Pipe Welded 37Ni-33Fe-23Cr-4Mo 45 45 ASTM/ASME B/SB-463 — N08026 80/35 [550/240] Plate, Material Number
183 AWS B2.1/B2.1M-BMG:2014 3W 0.6Cu-N -21.5Cr-3Mo-2.3Cu t Form Nominal Composition Welded TubeWelded 35Ni-30Fe-24Cr-6Mo-3Cu 170] Tube Welded 33Ni-42Fe-21Cr-Al-Ti 240] Forgings 42Ni-21.5Cr-3Mo-2.3Cu 750/380]690/310] Forgings Rod 33Cr-31Ni-32Fe-1.5Mo- 21Ni-30Fe-22Cr-18Co-3Mo- 550/240] Bar 35Ni-30Fe-24Cr-6Mo-3Cu 450/170] Forgings 33Ni-42Fe-21Cr-Al-Ti [515/240] Castings 42Ni [650/275] Forgings 31Ni-31Fe-27Cr-7Mo 35 [550/240] Bar 35Ni-35Fe-20Cr-Cb 40 [620/275]30 [515/205]25 [450/170] Forgings Forgings Forgings 37Ni-33Fe-25Cr 33Ni-42Fe-21Cr 33Ni-42Fe-21Cr Minimum Minimum Tensile/Yield Tensile/Yield 85/30 [585/205] Rod 47Ni-22Cr-19Fe-6Mo 90/35 [620/240] Rod 47Ni-22Cr-19Fe-6Mo Strength, ksi [MPa] Produc 0.75 3.5 89] ≤ 19] ≤ ≤ ≤ [mm] 8 and Diameter Diameter ≥ .2 (Continued) Thickness or [ [>19 and [>19 and (Continued) Limitations, in in Limitations, 0.3125 and 0.3125 ≥ Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 4545 45 45 ASTM/ASME ASTM/ASME B/SB-468 B/SB-468 — — N08024 N08026 80/35 [550/240] 80/35 [550/240] Tube Welded 37Ni-33Fe-23Cr-4Mo 4545 4545 4545 ASTM/ASME 4545 ASTM/ASME B/SB-473 8.2 ASTM/ASME B/SB-473 45 B/SB-473 ASTM — ASTM/ASME — A/SA-494 — CU5MCuC N08020 A479 N08024 N08826 N08026 904L N08904 80/ 80/35 [550/240] 75/35 80/35 [ Bar 71/31 [490/215] Bars & Shapes 37Ni-33Fe-23Cr-4Mo 44Fe-25Ni-21Cr-Mo 4545 4545 4545 ASTM/ASME 4545 ASTM/ASME B/SB-514 4545 ASTM/ASME B/SB-514 4545 ASTM/ASME B/SB-514 4545 — ASTM/ASME B/SB-515 4545 — ASTM/ASME B/SB-515 4545 — ASTM/ASME B/SB-515 45 N0812045 — ASTM/ASME B/SB-515 8.2 N0880045 — ASTM/ASME B/SB-564 45 N0881045 ASTM/ASME — B/SB-564 45 N0812045 — ASTM/ASME B/SB-564 44 N0880045 — ASTM/ASME B/SB-564 45 N08810 — ASTM/ASME B/SB-56445 45 N08811 — ASTM/ASME B/SB-564 90/40 [620/275] N08031 — ASTM/ASME B/SB-564 45 75/30 [515/205] N08120 — B/SB-564 65/25 [450/170] N08367 ASTM/ASME — Pipe Welded 90/40 [620/275] N08800 — B/SB-572 Pipe Welded 75/30 [515/205] N08810 — Pipe Welded 65/25 [450/170] N08811 Tube Welded 65/25 [450/ N08825 — Tube Welded 37Ni-33Fe-25Cr 94/40 R20033 Tube Welded 33Ni-42Fe-21Cr 90/ 95/45 [655/310] 33Ni-42Fe-21Cr R30556 37Ni-33Fe-25Cr 75/ 33Ni-42Fe-21Cr 65/ 33Ni-42Fe-21Cr 65/25 [ Forgings 85/35 [585/ 109/55 [ 46Fe-24Ni-21Cr-6Mo-Cu-N 100/45 [ 45 43 ASTM/ASME B/SB-581 — N06007 >0.75 and 45 43 ASTM/ASME B/SB-581 — N06007 Material Number
184 AWS B2.1/B2.1M-BMG:2014 3W 0.6Cu-N p 25Ni-47Fe-21Cr-5Mo rip 26Ni-22Cr-5Mo-Ti & Strip 47Ni-22Cr-20Fe-7Mo & Strip 47Ni-22Cr-19Fe-6Mo & Strip 47Ni-22Cr-20Fe-7Mo & Strip 47Ni-22Cr-19Fe-6Mo t Form Nominal Composition ate, Sheet, & Stri ate, Sheet, & Stripate, Sheet, & Strip 40Ni-29Cr-15Fe-5Mo 49Ni-25Cr-18Fe-6Mo Plate, Sheet, & St Seamless Pipe & TubeSeamless Pipe & Tube 47Ni-22Cr-19Fe-6Mo 40Ni-29Cr-15Fe-5Mo 0] Pipe Welded 21Ni-30Fe-22Cr-18Co-3Mo- 380] Pipe Welded 33Cr-31Ni-32Fe-1.5Mo- 35 [585/240]32 [585/220] Rod Rod 40Ni-29Cr-15Fe-5Mo 49Ni-25Cr-18Fe-6Mo Minimum Minimum Tensile/Yield Tensile/Yield 85/30 [585/205] Plate, Sheet, 85/30 [585/205] Plate, Sheet, 90/35 [620/240] Rod 47Ni-22Cr-20Fe-7Mo 85/30 [585/205] Rod 47Ni-22Cr-20Fe-7Mo Strength, ksi [MPa] Produc 0.75 2.5 2.5 3.5 64] 64] 89] ≤ 19] ≤ ≤ ≤ 19] 90/35 [620/240] Plate, Sheet, 19] 90/35 [620/240] Plate, Sheet, ≤ ≤ ≤ ≤ ≤ ≤ [mm] 8 and 0.75 [ 0.75 [ Diameter Diameter ≥ ≤ ≤ .2 (Continued) Thickness or [ [>19 and [>19 and [>19 and [>19 and [>19 and [>19 and (Continued) Limitations, in in Limitations, 0.3125 and 0.3125 ≥ Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 45 8.2 ASTM/ASME B/SB-599 — N08700 80/35 [550/240] Pl 45 45 ASTM/ASME B/SB-582 — N06985 45 45 ASTM/ASME B/SB-622 — N06030 85/35 [585/240] 4545 8.2 43 ASTM/ASME ASTM/ASME B/SB-621 B/SB-622 — — N08320 N06007 75/28 [515/195] 90/35 [620/240] Rod 26Ni-22Cr-5Mo-Ti 4545 4345 4545 ASTM/ASME 4545 ASTM/ASME B/SB-619 4545 ASTM/ASME B/SB-619 4545 ASTM/ASME B/SB-619 8.2 — ASTM/ASME B/SB-61945 45 ASTM/ASME — B/SB-619 — ASTM/ASME B/SB-61945 45 N06007 — B/SB-619 N06030 ASTM/ASME — 8.2 N06975 — B/SB-619 ASTM/ASME N06985 — B/SB-620 N08031 N08320 — R20033 — 90/35 [620/240] R30556 85/35 [585/240] 85/32 [585/220] N08320 Pipe Welded 90/35 [620/240] Pipe Welded 94/40 [650/275] Pipe Welded 75/28 [515/195] Pipe Welded 109/55 [750/ 47Ni-22Cr-19Fe-6Mo Pipe Welded 40Ni-29Cr-15Fe-5Mo Pipe Welded 100/45 [690/31 49Ni-25Cr-18Fe-6Mo 47Ni-22Cr-20Fe-7Mo 75/28 [515/195] 31Ni-31Fe-27Cr-7Mo 26Ni-22Cr-5Mo-Ti 4545 45 45 ASTM/ASME ASTM/ASME B/SB-582 B/SB-582 — — N06975 N06985 >0.75 and 85/32 [585/220] Pl 45 45 ASTM/ASME B/SB-582 — N06030 85/35 [585/240] Pl 4545 45 43 ASTM/ASME ASTM/ASME B/SB-581 B/SB-582 — — N08031 N06007 94/40 [650/275] Rod 31Ni-31Fe-27Cr-7Mo 45 45 ASTM/ASME45 B/SB-581 43 ASTM/ASME — B/SB-582 N06985 — N06007 >0.75 and 45 45 ASTM/ASME B/SB-581 — N06030 85/ 4545 45 45 ASTM/ASME ASTM/ASME B/SB-581 B/SB-581 — — N06975 N06985 >0.75 and 85/ Material Number
185 AWS B2.1/B2.1M-BMG:2014 3W 3W 0.6Cu-N 0.6Cu-N 0.6Cu-N p 31Ni-31Fe-27Cr-7Mo p 33Cr-31Ni-32Fe-1.5Mo- rip 44Fe-25Ni-21Cr-Mo t Form Nominal Composition less Pipe & Tube 37Fe-33Ni-26Cr-3Mo-Cu e, Sheet, & Strip 41Fe-25Ni-25Cr-5Mo-Cu-N ate, Sheet, & Stri ate, Sheet, & Stripate, Sheet, & Strip 25Ni-20Cr-6Mo-Cu-N ate, Sheet, & Stri 25Ni-20Cr-6Mo-Co-N amless Pipe & Tube 36Ni-35Fe-22Cr-5Mo-W amless Pipe & Tube 21Ni-30Fe-22Cr-18Co-3Mo- Plate, Sheet, & St Seamless Pipe & TubeSeamless Pipe & TubeSeamless Pipe & Tube 49Ni-25Cr-18Fe-6Mo 47Ni-22Cr-20Fe-7Mo 31Ni-31Fe-27Cr-7Mo Seamless Pipe & Tube 33Cr-31Ni-32Fe-1.5Mo- 0] Tube Welded 21Ni-30Fe-22Cr-18Co-3Mo- 380] Tube Welded 33Cr-31Ni-32Fe-1.5Mo- 195] Seamless Pipe & Tube 26Ni-22Cr-5Mo-Ti 620/240]585/240]585/220] Tube Welded 620/240] Tube Welded Tube Welded Tube Welded 47Ni-22Cr-19Fe-6Mo 40Ni-29Cr-15Fe-5Mo 49Ni-25Cr-18Fe-6Mo 47Ni-22Cr-20Fe-7Mo 650/275] Bar & Wire 31Ni-31Fe-27Cr-7Mo [490/215] Bar & Wire 44Fe-25Ni-21Cr-Mo Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 4545 4545 45 ASTM/ASME 45 ASTM/ASME B/SB-622 ASTM/ASME B/SB-622 B/SB-622 — — — N06985 N08031 N08135 90/35 [620/240] 94/40 [650/275] 73/31 [505/215] Se 45 45 ASTM/ASME B/SB-622 — N06975 85/32 [585/220] 4545 8.245 45 ASTM/ASME 45 ASTM/ASME B/SB-622 ASTM/ASME B/SB-622 B/SB-622 — — — N08320 N08535 R20033 75/28 [515/ 73/31 [505/215] 109/55 [750/380] Seam 45 45 ASTM/ASME B/SB-622 — R30556 100/45 [690/310] Se 45 45 ASTM/ASME B/SB-625 — N08031 94/40 [650/275] Pl 4545 8.245 8.2 ASTM/ASME45 45 ASTM/ASME B/SB-62545 ASTM/ASME B/SB-625 4345 B/SB-625 4545 ASTM/ASME — 4545 ASTM/ASME — B/SB-626 4545 ASTM/ASME B/SB-626 — 45 N0892645 ASTM/ASME B/SB-626 8.2 N08932 — ASTM/ASME B/SB-62645 45 ASTM/ASME R20033 — B/SB-626 — ASTM/ASME B/SB-62645 45 N06007 — B/SB-62645 N06030 ASTM/ASME — 4545 N06975 — B/SB-626 8.2 94/43 [650/295] ASTM/ASME N06985 — 8.2 ASTM/ASME 87/44 [600/305] N08031 B/SB-649 Pl ASTM/ASME N08320 109/55 [750/380] B/SB-649 — Plat B/SB-649 R20033 Pl 90/35 [ — — R30556 85/35 [ — 85/32 [ N08031 90/35 [ N08904 94/40 [650/275] N08925 75/28 [515/195] 109/55 [750/ Tube Welded Tube Welded 100/45 [690/31 94/40 [ 31Ni-31Fe-27Cr-7Mo 71/31 26Ni-22Cr-5Mo-Ti [600/295] 87/43 Bar & Wire 25Ni-20Cr-6Mo-Cu-N 45 8.2 ASTM/ASME B/SB-625 — N08925 87/43 [600/295] Pl 45 8.2 ASTM/ASME B/SB-625 — N08904 71/31 [490/215] Material Number
186 AWS B2.1/B2.1M-BMG:2014 0.6Cu-N 6Fe-24Ni-21Cr-6Mo-Cu-N t Form Nominal Composition Sheet, & Strip 46Fe-24Ni-21Cr-6Mo-Cu-N Welded PipeWelded 42Ni-21.5Cr-3Mo-2.3Cu Welded TubeWelded 42Ni-21.5Cr-3Mo-2.3Cu ate, Sheet, & Strip 31Ni-31Fe-29Cr-Mo ate, Sheet, & Strip 46Fe-24Ni-21Cr-6Mo Plate, Sheet, & Strip 4 Seamless Pipe & Tube 46Fe-24Ni-21Cr-6Mo Seamless Pipe & TubeSeamless Pipe & Tube 25Ni-20Cr-6Mo-Cu-N 25Ni-20Cr-6Mo-Cu-N 380] Bar & Wire 33Cr-31Ni-32Fe-1.5Mo- 310] Seamless Pipe & Tube 46Fe-24Ni-21Cr-6Mo-Cu-N 215] Seamless Pipe & Tube 44Fe-25Ni-21Cr-Mo 505/215] Seamless Tube 31Ni-31Fe-29Cr-Mo [550/240][490/215] Bar & Wire Pipe Welded 25Ni-47Fe-21Cr-5Mo [655/310] 44Fe-25Ni-21Cr-Mo Pipe Welded 46Fe-24Ni-21Cr-6Mo-Cu-N Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc 4.8] 100/45 [690/310] Seamless Pipe & Tube 46Fe-24Ni-21Cr-6Mo-Cu-N 4.8] 100/45 [690/310] Plate, 4.8] 100/45 [690/310] Tube Welded 46Fe-24Ni-21Cr-6Mo-Cu-N 4.8] 100/45 [690/310] Pipe Welded 46Fe-24Ni-21Cr-6Mo-Cu-N ≤ ≤ ≤ ≤ [mm] Diameter Diameter .2 (Continued) 0.1875 [ 0.1875 [ 0.1875 [ 0.1875 [ Thickness or (Continued) Limitations, in in Limitations, ≤ ≤ ≤ ≤ Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 4545 8.245 8.245 ASTM/ASME 4545 ASTM/ASME B/SB-691 45 ASTM/ASME B/SB-691 45 ASTM/ASME B/SB-704 — ASTM/ASME B/SB-705 — B/SB-709 — N08366 — N08367 — N08825 N08825 N08028[515/205] 75/30 [655/310] 95/45 & Wire Rod, Bar, 85/35 [585/240] & Wire Rod, Bar, 85/35 [585/240] 73/40 [505/275] 46Fe-24Ni-21Cr-6Mo 46Fe-24Ni-21Cr-6Mo-Cu-N Pl 4545 8.245 8.2 ASTM/ASME 8.2 ASTM/ASME B/SB-690 ASTM/ASME B/SB-690 B/SB-690 — — — N08366 N08367 N08367 >0.1875 [>4.8] 95/45 [655/ 75/30 [515/205] 45 8.2 ASTM/ASME B/SB-688 — N08367 >0.1875 [>4.8] 95/45 [655/310] 4545 8.245 8.245 ASTM/ASME 8.245 ASTM/ASME B/SB-676 8.245 ASTM/ASME B/SB-677 8.2 ASTM/ASME B/SB-677 8.2 — ASTM/ASME B/SB-677 — ASTM/ASME B/SB-688 — B/SB-688 N08367 — N08904 — >0.1875 [>4.8] N08925 — 95/45 [655/310] N08926 N08366 N08367 Tube Welded 46Fe-24Ni-21Cr-6Mo-Cu-N 71/31 [490/ 87/43 [600/295] 94/43 [650/295] 75/35 [515/240] Pl 45 8.2 ASTM/ASME B/SB-676 — N08367 4545 4545 8.245 ASTM/ASME 8.245 ASTM/ASME B/SB-668 8.245 ASTM/ASME B/SB-672 8.245 ASTM/ASME B/SB-673 8.245 ASTM/ASME — B/SB-673 8.245 — ASTM/ASME B/SB-673 8.245 — ASTM/ASME B/SB-674 8.2 N08028 — ASTM/ASME B/SB-674 N08700 8.2 — ASTM/ASME B/SB-674 N08904 — ASTM/ASME B/SB-675 N08925 — B/SB-675 N08926 — N08904 — N08925 — 73/31 [ N08926 80/35 N08367 71/31 N08367 >0.1875 [>4.8] 87/43 [600/295] 95/45 94/43 [650/295] 71/31 [490/215] Pipe Welded 87/43 [600/295] Pipe Welded 94/43 [650/295] Tube Welded Tube Welded 25Ni-20Cr-6Mo-Cu-N Tube Welded 25Ni-20Cr-6Mo-Cu-N 44Fe-25Ni-21Cr-Mo 25Ni-20Cr-6Mo-Cu-N 25Ni-20Cr-6Mo-Cu-N 4545 8.2 45 ASTM/ASME ASTM/ASME B/SB-649 B/SB-649 — — N08926 R20033[650/295] 94/43 109/55 [750/ Bar & Wire 25Ni-20Cr-6Mo-Cu-N Material Number
187 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition eet, & Strip 46Ni-26Cr-16Fe-3Mo-3W-3Co Sheet, & Strip 46Ni-22Cr-19Fe-9Mo-2W e, Sheet, & Strip 46Ni-27Cr-23Fe-2.75Si e, Sheet, & Strip 37Ni-30Co-28Cr-2.7Si amless Pipe & Tube 46Ni-27Cr-23Fe-2.75Si Rod, Bar, & WireRod, Bar, 46Ni-27Cr-23Fe-2.75Si Seamless Pipe & Tube 35Ni-35Fe-20Cr-Cb 205]185] Bars & Shapes Bars & Shapes 35Ni-19Cr-1.25Si 35Ni-19Cr-1.25Si-C 240] Seamless Tube 46Ni-27Cr-23Fe-2.75Si 620/240]620/240] Fittings620/240] Fittings Forgings 46Ni-27Cr-23Fe-2.75Si 37Ni-30Co-28Cr-2.7Si 46Ni-27Cr-23Fe-2.75Si 655/310] Pipe Welded 46Fe-24Ni-21Cr-6Mo-Cu-N [485/205] Fittings 35Ni-19Cr-1.25Si Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc 5] 100/45 [690/310] Pipe Welded Cold Worked 46Fe-24Ni-21Cr-6Mo-Cu-N 5] 100/45 [690/310] Pipe Welded 46Fe-24Ni-21Cr-6Mo-Cu-N 5] 100/45 [690/310] Pipe Welded 46Fe-24Ni-21Cr-6Mo-Cu-N ≤ ≤ ≤ [mm] Diameter Diameter 0.1875 [ 0.1875 [ 0.1875 [ .2 (Continued) Thickness or ≤ ≤ ≤ (Continued) Limitations, in in Limitations, Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 4646 4546 4546 ASTM/ASME 4646 ASTM/ASME B/SB-366 4646 ASTM/ASME B/SB-366 4546 ASTM/ASME B/SB-366 45 — ASTM/ASME B/SB-435 45 — ASTM/ASME B/SB-462 — ASTM/ASME B/SB-511 N06045 — B/SB-511 N08330 — N12160 — N12160 — N06045 N08330 N08332 90/35 [ 70/30 90/35 [ 90/35 [620/240] 90/35 [ Plat 70/30 [485/ 67/27 [460/ 4646 45 45 ASTM/ASME ASTM/ASME B/SB-167 B/SB-168 — — N06045 N06045 90/35 [620/240] 90/35 [620/240] Se Plat 4545 8.245 4345 4345 ASTM 4346 NACE 4346 NACE 45 A814 NACE MR 01-75 45 ASTM/ASME NACE MR 01-75 ASTM/ASME B/SB-163 MR 01-75 N08367 100 B/SB-166 MR 01-75 110 N08367 125 — N06950 140 [>5] >0.1875 — N06950 N06950 95/45 [655/310] N06045 Pipe Welded Cold Worked N06950 N06045 46Fe-24Ni-21Cr-6Mo-Cu-N [760/700] 110/102 [795/760] 115/110 [900/860] 131/125 90/35 [620/ 145/140 [1000/965] Pipe 90/35 [620/240] Pipe Pipe Pipe 50Ni-20Cr-18Fe-9Mo 50Ni-20Cr-18Fe-9Mo 50Ni-20Cr-18Fe-9Mo 50Ni-20Cr-18Fe-9Mo 4545 43 8.2 ASTM ASTM B814 A814 — N08367 N08367 N06920 95/35 [655/240] Plate, 4545 8.2 8.2 ASTM ASTM A813 A813 N08367 N08367 N08367 N08367 [>5] >0.1875 95/45 [655/310] Pipe Welded 46Fe-24Ni-21Cr-6Mo-Cu-N 4545 4345 —45 4345 ASTM 4345 ASTM 4345 ASTM 4545 B719 ASTM 8.2 B720 ASTM/ASME ASTM 8.2 ASTM/ASME B722 B/SB-729 ASTM/ASME B723 B/SB-804 — B726 B/SB-804 — — — — N06333 — — N08310 — N08020 N06333 N08367 N06333 N08367 N06333 [>5] >0.1875 95/45 [ 80/35 [550/240] 80/35 [550/240] 80/35 [550/240] [–/–] –/– 80/35 [550/240] Seamless Pipe & Tube 80/35 [550/240] Bar 46Ni-26Cr-16Fe-3Mo-3W-3Co Tube Seamless Pipe Welded Tube Welded 46Ni-26Cr-16Fe-3Mo-3W-3Co 46Ni-26Cr-16Fe-3Mo-3W-3Co 46Ni-26Cr-16Fe-3Mo-3W-3Co Fe-Cr-Ni-Mo 45 43 ASTM B718 — N06333 80/35 [550/240] Plate, Sh Material Number
188 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition e, Sheet, & Strip Co-26Cr-9Ni-5Mo-3Fe-2W ate, Sheet, & Stripate, Sheet, & Strip 35Ni-19Cr-1.25Si 35Ni-19Cr-1.25Si-C amless Pipe & Tube 37Ni-30Co-28Cr-2.7Si Seamless Pipe & TubeSeamless Pipe & Tube 35Ni-19Cr-1.25Si 35Ni-19Cr-1.25Si-C 240]240] Tube Welded Pipe Welded 46Ni-27Cr-23Fe-2.75Si 46Ni-27Cr-23Fe-2.75Si 620/240]620/240] Forgings Forgings 46Ni-27Cr-23Fe-2.75Si 37Ni-30Co-28Cr-2.7Si 485/205]460/185] Pipe Welded Pipe Welded 35Ni-19Cr-1.25Si 35Ni-19Cr-1.25Si-C Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or Limitations, in in Limitations, Table C Nickel and Nickel Base Alloys Nickel and Nickel UNS Number or Alloy or Alloy Designation Type, Grade, Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 4646 4546 4546 ASTM/ASME 4546 ASTM/ASME B/SB-517 4546 ASTM/ASME B/SB-535 4546 ASTM/ASME B/SB-535 4546 — ASTM/ASME B/SB-536 4646 — ASTM/ASME B/SB-536 4646 — ASTM/ASME B/SB-564 46 N06045 — ASTM/ASME B/SB-564 46 N08330 — ASTM/ASME B/SB-572 N08332 — ASTM/ASME B/SB-619 N08330 — B/SB-622 N08332 — N06045 — N12160 — 90/35 [620/ N12160 70/30 [485/205] N12160 67/27 [460/185] N12160 70/30 [485/205] 67/27 [460/185] Pl 90/35 [ Pl 90/35 [ 90/35 [620/240] 90/35 [620/240] 90/35 [620/240] Se Pipe Welded Rod 37Ni-30Co-28Cr-2.7Si 37Ni-30Co-28Cr-2.7Si 4646 45 45 ASTM/ASME ASTM B/SB-516 B512 — — N06045 N08330 90/35 [620/ 70/30 [485/205] Bars & Billets 35Ni-19Cr-1.25Si 4646 4646 4549 ASTM/ASME 4549 ASTM/ASME B/SB-626 — ASTM/ASME B/SB-710 — ASTM/ASME B/SB-710 — ASTM/ASME B/SB-815 — B/SB-818 — N12160 — N08330 — N08332 R31233 R31233 90/35 [620/240] 70/30 [ 67/27 [ Tube Welded 120/55 [825/380] 120/55 [825/380] Plat 37Ni-30Co-28Cr-2.7Si Rod Co-26Cr-9Ni-5Mo-3Fe-2W Material Number
189 AWS B2.1/B2.1M-BMG:2014 rip Ti-Ni-Pd-Ru-Cr & Strip Ti-0.5Ni-Ru & Strip Ti-0.3Co-Pd t, & Stript, & Stript, & Stript, & Strip Ti-Pd Ti-Pd Ti-Pd Ti-Pd t, & Stript, & Strip Ti-Pd Ti-Pd t Form Nominal Composition eet, & Strip Ti amless & Welded Pipeamless & Welded Ti-Pd Plate, Sheet, & St Seamless & Welded PipeSeamless & Welded PipeSeamless & Welded PipeSeamless & Welded Ti Ti-Pd Ti 170] Plate, Sheet, 275] Plate, Sheet, 240/140]240/140] Plate, Sheet, & Strip Plate, Shee Ti 345/275]400/275] Plate, Shee 240/140] Plate, Shee 345/275] Plate, Shee 345/275] Plate, Sheet, & Strip400/275] Plate, Sheet, & Strip240/140] Plate, Sheet, & Strip Plate, Sheet, & Strip Ti Ti-Ru Ti-Ru Ti-Ru 345/275]400/275] Plate, Shee Plate, Shee [400/275] Plate, Sh Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C UNS Titanium and Titanium Base Alloys and Titanium Titanium Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 51 51 ASTM/ASME B/SB-265 1 R50250 35/20 [ 51 51 ASTM/ASME B/SB-265 11 R52250 35/20 [ 5151 5251 5151 ASTM/ASME 5151 ASTM/ASME B/SB-265 5151 ASTM/ASME B/SB-265 5151 ASTM/ASME B/SB-265 5151 13 ASTM/ASME B/SB-265 5151 16 ASTM/ASME B/SB-265 51 16H ASTM/ASME B/SB-265 51 R53413 17 ASTM/ASME B/SB-265 R52402 ASTM/ASME 2 R52402 B/SB-265 26 B/SB-265 R52252 26H 27 R50400 R52404 2H R52404 40/25 [275/ R52254 50/40 [ R50400 58/40 [ 35/20 [ 50/40 [ 50/40 [ 58/40 [ 35/20 [ 58/40 51 52 ASTM/ASME B/SB-265 30 R53530 50/40 [345/ 5151 5451 5151 ASTM/ASME 5151 ASTM/ASME B/SB-265 5151 ASTM/ASME B/SB-265 5151 B/SB-265 5151 33 ASTM 5151 ASTM 7 5151 7H ASTM 51 R5344251 B337 ASTM/ASME ASTM 5251 B337 ASTM/ASME R52400 B/SB-338 R52400 5151 B337 ASTM/ASME B/SB-338 5151 B337 ASTM/ASME B/SB-338 1 5151 ASTM/ASME 1 B/SB-338 11 5151 11 ASTM/ASME B/SB-338 2 5151 13 ASTM/ASME B/SB-338 R50250 50/40 [345/275] 7 51 16 ASTM/ASME R50250 R52250 B/SB-338 51 R52250 16H 50/40 [ ASTM/ASME B/SB-338 58/40 [ R50400 R53413 17 ASTM/ASME B/SB-338 R52400 R52402 2 R52402 B/SB-338 26 R52252 26H 27 R50400 35/25 [240/170] R52404[240/140] 35/20 35/25 [240/170] R52404[240/140] 35/20 Tube Seamless & Welded 50/40 [345/275] Tube Seamless & Welded [275/170] 40/25 R52254 50/40 [345/275]Tube Seamless & Welded [345/275] 50/40 [400/275] 58/40 Se Tube Seamless & Welded Tube Seamless & Welded [240/140] 35/20 Ti Ti-Pd Ti-0.5Ni-Ru Tube Seamless & Welded [345/275] 50/40 [345/275] 50/40 Tube Seamless & Welded [400/275] 58/40 Ti-Pd Tube Seamless & Welded Ti-Pd Tube Seamless & Welded [240/140] 35/20 Ti-Pd Tube Seamless & Welded Ti Ti-Ru Ti-Ru Ti-Ru Material Number
190 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition 170] FittingsWelded Seamless & Ti-0.5Ni-Ru 275] FittingsWelded Seamless & Ti-0.3Co-Pd 345/275] Bars & Billets240/170] FittingsWelded Seamless & 345/275] FittingsWelded Ti-Ni-Pd-Ru-Cr Seamless & 400/275] FittingsWelded Seamless & 240/170] Ti-Pd FittingsWelded Seamless & 345/275] Ti-Pd FittingsWelded Seamless & 400/275] Ti-Pd FittingsWelded Seamless & Ti-Pd Ti-Ru Ti-Ru [275/170] Bars & Billets Ti-0.5Ni-Ru [345/275] Bars & Billets[240/170] FittingsWelded Seamless & Ti-0.3Co-Pd Ti [345/275] FittingsWelded Seamless & Ti Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C UNS Titanium and Titanium Base Alloys and Titanium Titanium Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 5151 5151 5251 ASTM/ASME 5451 ASTM/ASME B/SB-338 5151 ASTM/ASME B/SB-338 5151 ASTM/ASME B/SB-338 5151 2H ASTM/ASME B/SB-338 51 30 ASTM/ASME B/SB-338 52 33 ASTM/ASME B/SB-348 R50400 ASTM/ASME 7 B/SB-348 R53530 7H B/SB-348 R53442 1 11 R52400 R52400 13 R50250 R52250[400/275] 58/40 R53413Tube Seamless & Welded [345/275] 50/40 Tube Seamless & Welded [345/275] 50/40 Tube Seamless & Welded [345/275] 50/40 [400/275] 58/40 Tube Seamless & Welded Tube Seamless & Welded Ti-0.3Co-Pd Ti Ti-Ni-Pd-Ru-Cr 35/20 [240/140] 35/20 [240/140] 40/25 Bars & Billets Ti-Pd Bars & Billets Ti-Pd Ti Ti-Pd 5151 5151 5151 ASTM/ASME 5151 ASTM/ASME B/SB-348 5151 ASTM/ASME B/SB-348 5151 ASTM/ASME B/SB-348 5151 16 ASTM/ASME B/SB-348 51 16H51 ASTM/ASME B/SB-348 5251 17 ASTM/ASME B/SB-348 54 R5240251 ASTM/ASME 2 R52402 B/SB-348 5151 26 ASTM/ASME B/SB-348 51 R52252 26H51 ASTM/ASME B/SB-348 5151 2H ASTM/ASME R50400 B/SB-348 51 R5240451 30 ASTM/ASME R52404 B/SB-348 5251 33 ASTM/ASME B/SB-363 R50400 5151 ASTM/ASME 7 B/SB-363 50/40 [345/275] 51 R5353051 7H ASTM/ASME 58/40 [400/275] B/SB-363 WPT 1 51 R5344251 ASTM/ASME WPT 11 B/SB-363 35/20 [240/140] 5151 ASTM/ASME R52400 Bars & Billets WPT 13 B/SB-363 R50250 R52400 Bars & Billets 5151 50/40 [345/275] ASTM/ASME R52250 WPT 16 B/SB-363 50/40 [345/275] 51 WPT 16H ASTM/ASME 58/40 [400/275] Bars & Billets R53413 B/SB-363 52 ASTM/ASME R52402 WPT 17 B/SB-363 58/40 [400/275] Bars & Billets R52402 ASTM/ASME Bars & Billets B/SB-363 WPT 2 50/40 Bars & Billets R52252 WPT 26 B/SB-363 50/40 [ Ti-Pd Bars & Billets WPT 26H Ti-Pd R50400 50/40 [345/275] R52404 WPT 30 35/25 58/40 [400/275] Ti-Pd R52404[ 35/25 [275/ 40/25 R53530 Ti Bars & Billets Ti-Ru [ 50/40 Bars & Billets Ti-Ru [ 58/40 Ti [ 35/25 50/40 [ 50/40 [ 58/40 Ti-Pd Ti-Pd [345/ 50/40 Material Number
191 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition 345/275] FittingsWelded Seamless & 400/275] FittingsWelded Seamless & Ti-Pd Ti-Pd [275/170] Seamless Pipe Ti-0.5Ni-Ru Minimum Minimum Tensile/Yield Tensile/Yield 50/40 [345/275]40/25 [275/170] Castings Forgings Ti-Pd 50/40 [345/275] Ti-0.5Ni-Ru Forgings Ti-0.3Co-Pd Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, 402252250 50/40 [345/275]402 35/25 [240/170]402252 Castings Castings 35/20 [240/140] 50/40 [345/275] 58/40 [400/275]400 Forgings 35/20 [240/140]400 Ti-Pd Forgings Ti-Pd Forgings Forgings Ti-Pd 50/40 [345/275] 58/40 [400/275] Ti-Pd Ti-Pd Forgings Ti-Pd Forgings Ti-Pd Ti-Pd Table C 50400 50/40 [345/275] Castings Ti UNS Titanium and Titanium Base Alloys and Titanium Titanium Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 5151 5151 5151 ASTM/ASME 5151 ASTM/ASME B/SB-363 5151 ASTM/ASME B/SB-367 5151 ASTM/ASME WPT 7H B/SB-367 5151 ASTM/ASME B/SB-367 C-16 5151 R52400 ASTM/ASME B/SB-367 C-17 5251 ASTM/ASME B/SB-381 5151 C-2 ASTM/ASME R52 B/SB-381 5151 C-7 ASTM/ASME R52 B/SB-381 5151 F-1 ASTM/ASME B/SB-381 R 51 F-1151 ASTM/ASME B/SB-381 51 F-1351 ASTM/ASME — B/SB-381 R50250 51 F-16 58/40 [ 51 ASTM/ASME R52 B/SB-381 F-16H 5151 ASTM/ASME R53413 B/SB-381 52 F-1751 ASTM/ASME R52 B/SB-381 R52 5151 F-2 ASTM/ASME B/SB-381 51 F-2651 ASTM/ASME R52 B/SB-381 F-26H 5151 ASTM/ASME B/SB-381 R50400 F-2H 5151 ASTM/ASME R52404 B/SB-381 35/20 [240/140] R52404 52 F-3051 ASTM/ASME B/SB-861 5151 F-7 R50400 ASTM/ASME B/SB-861 F-7H 5151 ASTM/ASME R53530 B/SB-861 Forgings 5151 ASTM/ASME 1 B/SB-861 R52 5151 R52 11 ASTM/ASME B/SB-861 5151 13 ASTM/ASME B/SB-861 50/40 [345/275] 51 50/40 [345/275] 16 ASTM/ASME R50250 B/SB-861 58/40 [400/275] 51 R52250 16H ASTM/ASME B/SB-861 R53413 58/40 [400/275] 17 ASTM/ASME B/SB-861 Forgings R52402 2 Forgings R52402 B/SB-861 Ti Forgings 26 R52252 26H Forgings 2H R50400 R52404 35/20 [240/140] R52404 35/20 [240/140] 40/25 R50400 Ti Seamless Pipe Ti-Ru 50/40 [345/275] Ti-Ru 58/40 [400/275] Seamless Pipe 35/20 [240/140] Ti Seamless Pipe Seamless Pipe 50/40 [345/275] 50/40 [345/275] 58/40 [400/275] Seamless Pipe Ti 58/40 [400/275] Seamless Pipe Ti-Pd Seamless Pipe Seamless Pipe Ti-Pd Seamless Pipe Ti-Pd Ti-Pd Ti Ti-Ru Ti-Ru Ti 51 51 ASTM/ASME B/SB-363 WPT 7 R52400 50/40 [ Material Number
192 AWS B2.1/B2.1M-BMG:2014 rip Ti-0.3Mo-0.8Ni rip Ti-Ni-Pd-Ru-Cr & Strip& Strip& Strip Ti-0.5Ni-Ru Ti-0.5Ni-Ru Ti-0.3Co-Pd t Form Nominal Composition less & Welded Pipeless & Welded Ti-0.3Mo-0.8Ni Plate, Sheet, & St Plate, Sheet, & St Seamless & Welded PipeSeamless & Welded Ti 275]380] Plate, Sheet, Plate, Sheet, 380] Plate, Sheet, 450/380] Plate, Sheet, & Strip Ti [275/170] Pipe Welded Ti-0.5Ni-Ru Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C UNS Titanium and Titanium Base Alloys and Titanium Titanium Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 5151 5451 5151 ASTM/ASME 5151 ASTM/ASME B/SB-861 5151 ASTM/ASME B/SB-861 51 ASTM/ASME B/SB-861 52 33 ASTM/ASME B/SB-862 ASTM/ASME 7 B/SB-862 7H B/SB-862 R53442 1 11 R52400 R52400 13 R50250 R52250 R53413 50/40 [345/275] 50/40 [345/275] 58/40 [400/275] Seamless Pipe 35/20 [240/140] Seamless Pipe 35/20 [240/140] Seamless Pipe 40/25 Pipe Welded Ti-Ni-Pd-Ru-Cr Pipe Welded Ti-Pd Ti-Pd Ti Ti-Pd 5151 5151 5151 ASTM/ASME 5151 ASTM/ASME B/SB-862 5151 ASTM/ASME B/SB-862 5151 ASTM/ASME B/SB-862 5151 16 ASTM/ASME B/SB-862 51 16H51 ASTM/ASME B/SB-862 5151 17 ASTM/ASME B/SB-862 54 R5240251 ASTM/ASME 2 R52402 B/SB-862 5152 26 ASTM/ASME B/SB-862 51 R52252 26H52 ASTM/ASME B/SB-862 5252 27 ASTM/ASME R50400 B/SB-862 52 R5240452 2H ASTM/ASME R52404 B/SB-862 5252 33 ASTM/ASME B/SB-265 52 R5225452 ASTM/ASME 7 B/SB-265 50/40 [345/275] R50400 5252 7H ASTM/ASME 58/40 [400/275] B/SB-265 54 R53442 12 ASTM/ASME B/SB-265 35/20 [240/140] 52 14 ASTM/ASME R52400 B/SB-265 Pipe Welded R52400 Pipe Welded 50/40 [345/275] 15 B/SB-265 50/40 [345/275] R53400 58/40 [400/275] ASTM 3 Pipe Welded R53414 31 35/20 [240/140] Pipe Welded R53415 34 Pipe Welded 58/40 [400/275] Pipe Welded B337 R50550 50/40 [345/275] R53532 Ti-Pd Pipe Welded Ti-Pd R53445 50/40 [345/275] Pipe Welded 58/40 [400/275] Ti-Pd Pipe Welded 12 70/50 [485/345] 60/40 [415/ Pipe Welded Ti Ti-Ru Pipe Welded Ti-Ru 70/55 [485/ R53400 65/55 [ Ti-Ru Ti-Ni-Pd-Ru-Cr 65/55 [450/ Ti 65/55 [450/380] Ti-Pd Ti-Pd 70/50 [485/345] Seam 52 52 ASTM B337 3 R50550 65/55 [450/380] 5252 5252 5252 ASTM/ASME 52 ASTM/ASME B/SB-338 52 ASTM/ASME B/SB-338 ASTM/ASME B/SB-338 12 B/SB-338 14 15 R53400 3 R53414 R53415 R50550[485/345] 70/50 Tube Seamless & Welded [415/275] 60/40 Tube Seamless & Welded [485/380] 70/55 Tube Seamless & Welded Ti-0.3Mo-0.8Ni [450/380] 65/55 Tube Seamless & Welded Ti-0.5Ni-Ru Ti-0.5Ni-Ru Ti Material Number
193 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition Seamless & Welded FittingsWelded Seamless & Ti-0.3Mo-0.8Ni 275] FittingsWelded Seamless & 380] FittingsWelded Seamless & Ti-0.5Ni-Ru Ti-0.5Ni-Ru 485/345] Bars & Billets450/380] Ti-0.3Mo-0.8Ni Bars & Billets Ti-Ni-Pd-Ru-Cr [450/380] FittingsWelded Seamless & Ti [415/275][485/380] Seamless Pipe Seamless Pipe[415/275][485/380] Ti-0.5Ni-Ru Pipe Welded Ti-0.5Ni-Ru Pipe Welded Ti-0.5Ni-Ru Ti-0.5Ni-Ru [415/275][485/380] Bars & Billets[450/380] Bars & Billets Bars & Billets Ti-0.5Ni-Ru Ti-0.5Ni-Ru Ti-0.3Co-Pd 50 [485/345] Forgings Ti-0.3Mo-0.8Ni Minimum Minimum Tensile/Yield Tensile/Yield 65/55 [450/380]60/40 [415/275]70/55 [485/380] Castings65/55 [450/380] Forgings Forgings Forgings Ti-Pd Ti-0.5Ni-Ru Ti-0.5Ni-Ru Ti-0.3Co-Pd Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C 50550 65/55 [450/380] Castings Ti UNS Titanium and Titanium Base Alloys and Titanium Titanium Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 5252 5252 5252 ASTM/ASME 5252 ASTM/ASME B/SB-363 5252 ASTM/ASME B/SB-363 5252 ASTM/ASME WPT 14 B/SB-363 5252 ASTM/ASME WPT 15 B/SB-367 5252 ASTM/ASME R53414 B/SB-367 WPT 3 5252 ASTM/ASME R53415 B/SB-381 5252 C-3 ASTM/ASME B/SB-381 R50550 5252 C-8 ASTM/ASME B/SB-381 52 F-1252 ASTM/ASME B/SB-381 R 52 F-1452 ASTM/ASME B/SB-381 52 F-1552 ASTM/ASME R53400 — B/SB-861 5252 F-3[415/ 60/40 ASTM/ASME R53414 B/SB-861 54 F-3152[450/ 65/55 ASTM/ASME R53415 B/SB-861 5252 12 ASTM/ASME B/SB-861 65/55 R50550 5252 14 ASTM/ASME R53532 B/SB-861 5252 15 ASTM/ASME B/SB-862 52 R53400 ASTM/ASME 3 B/SB-862 54 R53414 70/ 34 ASTM/ASME B/SB-862 R53415 12 ASTM/ASME B/SB-862 14 R50550 B/SB-862 R53445 15 65/55 [450/380] R53400 3 R53414 34 70/50 [485/345] R53415 60/40 Forgings R50550 70/55 R53445 Seamless Pipe 65/55 [450/380] 65/55 [450/380] 70/50 [485/345] Seamless Pipe 60/40 Seamless Pipe Ti-0.3Mo-0.8Ni 70/55 Pipe Ti Welded 65/55 [450/380] 65/55 [450/380] Ti-Ni-Pd-Ru-Cr Pipe Welded Pipe Welded Ti Ti-0.3Mo-0.8Ni Ti-Ni-Pd-Ru-Cr Ti 5252 5252 5252 ASTM/ASME 5252 ASTM/ASME B/SB-348 5252 ASTM/ASME B/SB-348 54 ASTM/ASME B/SB-348 52 14 ASTM/ASME B/SB-348 15 ASTM/ASME B/SB-348 3 B/SB-363 R53414 31 R53415 34 WPT 12 R50550 R53532 R53400 R53445 60/40 70/55 65/55 [450/380] 65/55 [485/345] 70/50 65/55 [ Bars & Billets Ti 5252 5252 54 ASTM/ASME 52 ASTM/ASME B/SB-338 ASTM/ASME B/SB-338 B/SB-348 31 34 12 R53532 R53445 R53400[450/380] 65/55 Tube Seamless & Welded [450/380] 65/55 Tube Seamless & Welded 70/50 [ Ti-0.3Co-Pd Ti-Ni-Pd-Ru-Cr Material Number
194 AWS B2.1/B2.1M-BMG:2014 i-5Al-1Sn-1Zr-1V-Mo p Ti-15Mo-3Al-2.7Nb-Si rip Ti-3Al-2.5V-Pd Strip Ti-3Al-2.5V t Form Nominal Composition eet, & Strip Ti e, Sheet, & Strip Ti-3Al-8V-6Cr-4Zr-4Mo-Pd less & Welded Pipeless & Welded Ti-3Al-2.5V ate, Sheet, & Strip Ti-3Al-8V-6Cr-4Zr-4Mo ate, Sheet, & Stripate, Sheet, & Strip Ti-3Al-2.5V-0.1Ru T Plate, Sheet, & St Plate, Sheet, & Stri Plate, Sheet, & amless & Welded FittingsWelded amless & Ti-3Al-8V-6Cr-4Zr-4Mo FittingsWelded amless & Ti-3Al-8V-6Cr-4Zr-4Mo-Pd FittingsWelded amless & Ti-3Al-2.5V-0.1Ru Seamless & Welded FittingsWelded Seamless & Ti-3Al-2.5V-Pd FittingsWelded Seamless & Ti-15Mo-3Al-2.7Nb-Si FittingsWelded Seamless & Ti-3Al-2.5V 5] Bars & Billets Ti-5Al-1Sn-1Zr-1V-Mo /760] Bars & Billets Ti-15Mo-3Al-2.7Nb-Si 485] Bars & Billets Ti-3Al-2.5V-0.1Ru 795/760] Forgings Ti-3Al-8V-6Cr-4Zr-4Mo-Pd 620/485] Bars & Billets Ti-3Al-2.5V [550/485] Plate, Sh 70 [620/485] Forgings Ti-3Al-2.5V-Pd Minimum Minimum Tensile/Yield Tensile/Yield 80/70 [550/485] Bars & Billets Ti Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C UNS Titanium and Titanium Base Alloys and Titanium Titanium Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 53 53 ASTM/ASME B/SB-265 18 R56322 90/70 [620/485] 53 54 ASTM/ASME B/SB-265 19 R58640 [795/760] 115/110 Pl 5353 54 54 ASTM/ASME ASTM/ASME B/SB-265 B/SB-265 20 21 R58645 R58210 [795/760] 115/110 [795/760] 115/110 Plat 53 5453 ASTM/ASME B/SB-363 535353 ASTM/ASME WPT 19 5353 B/SB-363 54 ASTM/ASME R58640 54 ASTM/ASME WPT 28 B/SB-381 ASTM/ASME B/SB-381 R56323 B/SB-381 F-18 F-19 F-20 R56322 [795/760] 115/110 Se R58640 R58645[620/485] 90/70 Se 90/ [795/760] 115/110 [ 115/110 Forgings Ti-3Al-8V-6Cr-4Zr-4Mo 5353 5353 5253 ASTM/ASME 51.453 ASTM/ASME B/SB-265 ASTM/ASME 5353 B/SB-265 53 B/SB-26553 ASTM/ASME 5353 28 B/SB-265 5353 32 ASTM/ASME ASTM 4 5353 ASTM/ASME B/SB-338 53 R5632353 ASTM/ASME 9 B/SB-338 54 R5511153 B337 ASTM/ASME B/SB-338 R50700 5453 18 ASTM/ASME B/SB-348 5453 28 ASTM/ASME R56320 B/SB-348 5353 ASTM/ASME 9 B/SB-348 9 52 R5632253 18 ASTM/ASME B/SB-348 51.4 R5632353 19 ASTM/ASME B/SB-348 ASTM/ASME 90/70 [620/485] 53 20 R56320 B/SB-348 100/85 [690/585] R56320 53 B/SB-348 R5632253 21 ASTM/ASME Pl 80/70 R5864053 Pl 28 ASTM/ASME B/SB-348 54 R58645 90/70 [620/485] 32 B/SB-363 4 54 R5821053 ASTM/ASME[620/485] 90/70 R56323 ASTM/ASME 9 WPT 18 B/SB-363Tube Seamless & Welded [620/485] 90/70 53 R55111 B/SB-363Tube Seamless & Welded R50700 [620/485] 90/70 ASTM/ASME R56322 WPT 20 90/70 [620/485] 90/70 [620/485]Tube Seamless & Welded Ti-3Al-2.5V-Pd R56320 [795/760] 115/110 WPT 21 B/SB-363 Seam Ti-3Al-2.5V-0.1Ru R58645 115/110 [795/760] Bars & Billets R58210 [795 115/110 WPT 9 Bars & Billets Ti-3Al-2.5V Bars & Billets 90/70 [620/ 100/85 [690/58 R56320 Ti-3Al-8V-6Cr-4Zr-4Mo Ti-3Al-8V-6Cr-4Zr-4Mo-Pd [620/485] 90/70 Ti-3Al-2.5V-Pd 90/70 [ [795/760] 115/110 Se [795/760] 115/110 90/70 [620/485] Material Number
195 AWS B2.1/B2.1M-BMG:2014 -15Mo-3Al-2.7Nb-Si Al-8V-6Cr-4Zr-4Mo-Pd ube Ti-4Al-2.5V-1.5Fe p Ti-6Al-4V-Pd-ELI-Ru rip Ti-4Al-2.5V-1.5Fe Strip Ti-6Al-4V-Pd Strip Ti-5Al-2.5Sn pe Ti-3Al-2.5V & Strip Ti-6Al-4V t Form Nominal Composition Plate, Sheet, & Stri Plate, Sheet, & St Seamless & Welded T Seamless & Welded 760]760] Seamless Pipe Seamless Pipe Ti-3Al-8V-6Cr-4Zr-4Mo Ti-3 825] Plate, Sheet, & 825] Plate, Sheet, & Strip795] Ti-6Al-4V-Ni-Pd Plate, Sheet, & /760] Seamless Pipe Ti /825] Plate, Sheet, /825] Bars & Billets Ti-4Al-2.5V-1.5Fe 825/760]895/825] Bars & Billets Bars & Billets Ti-6Al-4V-ELI Ti-6Al-4V-Pd [795/760] Forgings Ti-15Mo-3Al-2.7Nb-Si 620/485] Seamless Pi 620/485] Seamless Pipe Ti-3Al-2.5V-Pd [620/485] Forgings Ti-3Al-2.5V-0.1Ru [620/485] Pipe Welded Ti-3Al-2.5V-Pd Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, Table C UNS Titanium and Titanium Base Alloys and Titanium Titanium Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 5353 5453 53 ASTM/ASME 53 ASTM/ASME B/SB-861 ASTM/ASME B/SB-861 B/SB-861 21 28 9 R58210 R56323 R56320 [795 115/110 90/70 [620/485] 90/70 [ Seamless Pipe Ti-3Al-2.5V-0.1Ru 53 54 ASTM/ASME B/SB-381 F-21 R58210 115/110 5353 5353 51.453 ASTM/ASME ASTM/ASME 5353 B/SB-381 53 B/SB-38153 ASTM/ASME 54 ASTM/ASME B/SB-381 54 F-28 ASTM/ASME B/SB-861 F-4 ASTM/ASME B/SB-86153 F-9 R56323 B/SB-86153 R50700 18 5353 19 R56320 5453 20 ASTM/ASME 54 R5632253 ASTM/ASME B/SB-862 54 R5864053 ASTM/ASME B/SB-862 53 R5864553 ASTM/ASME B/SB-862 5354 90/70 18 ASTM/ASME B/SB-862 54 80/70 [550/485] 19 ASTM/ASME B/SB-862 53 20 B/SB-862 90/70 [620/485] R56322 21 ASTM/ASME AMS 90/70 [ R58640 28 Forgings [795/ 115/110 B/SB-265 R58645 9 [795/ 115/110 Forgings R58210 4914 R56323 24 R56320 90/70 R56405 — [795/760] 115/110 Ti Ti-3Al-2.5V [795/760] 115/110 [795/760] 115/110 Pipe Welded R58153 90/70 [620/485]Pipe Welded Pipe Welded 90/70 [620/485] Ti-3Al-8V-6Cr-4Zr-4Mo Ti-3Al-8V-6Cr-4Zr-4Mo-Pd [895/ 130/120 Pipe Welded Pipe Welded Ti-15Mo-3Al-2.7Nb-Si 98/96 [675/660] Ti-3Al-2.5V-0.1Ru Ti-3Al-2.5V Sheet Ti-15V-3Al-3Cr-3Sn 5454 53 53 ASTM/ASME54 ASTM/ASME B/SB-26554 B/SB-265 52 53 25 ASTM/ASME 29 ASTM/ASME B/SB-265 B/SB-338 R56403 R56404 6 35 R54520 R56340 [895/ 130/120 [825/760] 120/110 [825/ 120/115 [895/825] 130/120 54 53 ASTM/ASME B/SB-265 5 R56400 [895 130/120 54 53 ASTM/ASME B/SB-265 35 R56340 [895/825] 130/120 5454 5354 5354 ASTM/ASME 5354 ASTM/ASME B/SB-348 53 ASTM/ASME B/SB-348 53 ASTM/ASME B/SB-348 23 ASTM/ASME B/SB-348 24 B/SB-348 25 R56407 35 R56405 5 R56403 R56340 R56400 [ 120/110 [ 130/120 130/120 [895/825] [895 130/120 Bars & Billets 130/120 [895/825] Bars & Billets Ti-6Al-4V-Ni-Pd Ti-6Al-4V Material Number
196 AWS B2.1/B2.1M-BMG:2014 Ti-4Al-2.5V-1.5Fe pe Ti-6Al-4V-ELI t Form Nominal Composition 760] FittingsWelded Seamless & 825] FittingsWelded Seamless & Ti-6Al-4V-ELI Ti-6Al-4V-Ni-Pd /825] FittingsWelded Seamless & Ti-6Al-4V-Pd /760]/825] Seamless Pipe Seamless Pipe Ti-6Al-4V-Pd-ELI-Ru 825/795] Bars & Billets Ti-5Al-2.5Sn 825/760] Seamless Pi 895/825] Seamless Pipe Ti-6Al-4V-Ni-Pd [895/825] Seamless Pipe Ti-6Al-4V [895/825] Forgings Ti-6Al-4V-Ni-Pd 120 [895/825]120 Forgings Ti-6Al-4V-Pd Minimum Minimum Tensile/Yield Tensile/Yield 130/120 [895/825]130/120 Plate Ti-8Al-1Mo-1V 120/110 [825/760]120/110 Plate Ti-8Al-1Mo-1V Strength, ksi [MPa] Produc 145/135 [1000/930] Plate Ti-8Al-1Mo-1V 0.5 4 65] ≤ ≤ 13] 100] 2.5 ≤ ≤ ≤ ≤ [mm] Diameter Diameter .2 (Continued) Thickness or [>5 and [>25 and [>25 and (Continued) Limitations, in in Limitations, [>65 and Table C UNS Titanium and Titanium Base Alloys and Titanium Titanium Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 5454 5354 5354 ASTM/ASME 5354 ASTM/ASME B/SB-363 5354 ASTM/ASME B/SB-363 5254 ASTM/ASME WPT 23 B/SB-363 5354 ASTM/ASME WPT 24 B/SB-367 5354 ASTM/ASME R56407 WPT 25 B/SB-367 5354 ASTM/ASME R56405 B/SB-381 5354 C-5 ASTM/ASME R56403 B/SB-381 52 C-6 ASTM/ASME B/SB-381 53 F-23 ASTM/ASME B/SB-381 R56400 F-24 ASTM/ASME B/SB-381 R54520 F-25 R56407 B/SB-861 [825/ 120/110 F-5 R56405 [895 130/120 F-6 R56403 [895/ 130/120 23 R56400 R54520 [895/825] 130/120 R56407 [795/725] 115/105 [825/760] 120/110 130/ Castings 130/120 Castings Forgings [895/825] 130/120 [825/795] 120/115 [ 120/110 Forgings Ti-6Al-4V Forgings Ti-5Al-2.5Sn Ti-6Al-4V-ELI Ti-6Al-4V Ti-5Al-2.5Sn 54 52 ASTM/ASME B/SB-348 6 R54520 [ 120/115 5454 5354 5354 ASTM/ASME 53 ASTM/ASME B/SB-861 53 ASTM/ASME B/SB-861 ASTM/ASME B/SB-861 24 B/SB-861 25 29 R56405 35 R56403 R56404 R56340 [895/825] 130/120 [ 130/120 [825 120/110 Pipe Seamless [895 130/120 Ti-6Al-4V-Pd 5454 5354 5354 ASTM/ASME 5354 ASTM/ASME B/SB-861 5354 ASTM/ASME B/SB-862 5354 ASTM/ASME B/SB-862 5354 ASTM/ASME 5 B/SB-862 53 23 ASTM/ASME B/SB-86254 52 24 ASTM/ASME B/SB-862 25 R56400 B/SB-862 52 R56407 29 AMS R56405 35 R56403 AMS 5 R56404 4915 R56340 R56400 4915 130/120 [825/760] 120/110 — [895/825] 130/120 [895/825] 130/120 Pipe Welded — [825/760] 120/110 Pipe Welded R54810 [895/825] 130/120 Pipe Welded and >0.187 R54810 [895/825] 130/120 Pipe Welded Pipe Welded Ti-6Al-4V-ELI >2.5 and Pipe Welded Ti-6Al-4V-Pd Ti-6Al-4V-Ni-Pd Ti-6Al-4V-Pd-ELI-Ru Ti-4Al-2.5V-1.5Fe Ti-6Al-4V 54 52 AMS 4915 — R54810 >1 and Material Number
197 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition Minimum Minimum Tensile/Yield Tensile/Yield 140/130 [965/895]140/130 Plate Ti-8Al-1Mo-1V 120/110 [825/760]120/110 Forgings Ti-8Al-1Mo-1V Strength, ksi [MPa] Produc 4 1 5] 145/135 [1000/930] Sheet & Strip Ti-8Al-1Mo-1V 25] ≤ ≤ 100] ≤ ≤ 65] [895/825] 130/120 Forgings Ti-8Al-1Mo-1V ≤ ≤ [mm] 2.5 [ 0.187 [ 0.187 Diameter Diameter ≤ ≤ .2 (Continued) Thickness or [>13 and [>13 and Limitations, in in Limitations, [>65 and Table C UNS Titanium and Titanium Base Alloys and Titanium Titanium Number Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 5454 5254 52 52 AMS AMS AMS 4915 4919 4973 — — — R54810 R54620 R54810 >2.5 and [930/860] 135/125 Sheet Ti-6Al-4Zr-2Mo-2Sn 54 52 AMS 4915 — R54810 >0.5 and 54 52 AMS 4973 — R54810 5454 52 52 AMS AMS 4975 4976 — — R54620 R54620 [895/825] 130/120 [895/825] 130/120 Bar Forgings Ti-6Al-4Zr-2Mo-2Sn Ti-6Al-4Zr-2Mo-2Sn Material Number
198 AWS B2.1/B2.1M-BMG:2014 1.45Sn-0.28(Fe+Ni+Cr) 97.5Zr-1.5Sn-0.3(Fe+Cr) rip 97.3Zr-2.6Cb StripStrip 95.5Zr+2.5Cb 95.5Zr+2.5Cb & Strip 99.9Zr t, & Strip 99.2Zr t Form Nominal Composition Welded PipeWelded 99.2Zr Sheet, & Strip 98Zr- eet & Strip 98.2Zr-1.5Sn-0.32(Fe+Cr) Rod, & Wire Rod, & Wire 98Zr-1.45Sn-0.28(Fe+Ni+Cr) 98.2Zr-1.5Sn-0.32(Fe+Cr) ss & Welded Tube ss & Welded 98Zr-1.45Sn-0.28(Fe+Ni+Cr) Tube ss & Welded 98.2Zr-1.5Sn-0.32(Fe+Cr) ate, Sheet, & St ate, Sheet, & Strip amless & Welded Tube amless & Welded 97.5Zr-1.5Sn-0.3(Fe+Cr) 140] Plate, Sheet, 380]345] Plate, Sheet, & Plate, Sheet, & 380/205] FittingsWelded Seamless & 99.2Zr 550/380]Tube Seamless & Welded 415/240] 95.5Zr+2.5Cb Bar & Wire 97.5Zr-1.5Sn-0.3(Fe+Cr) [380/205] Plate, Shee [380/205] Seamless & [415/240] Forgings 97.5Zr-1.5Sn-0.3(Fe+Cr) Minimum Minimum Tensile/Yield Tensile/Yield 70/55 [485/380] Forgings[550/380]80/55 Bar & Wire 95.5Zr+2.5Cb 95.5Zr+2.5Cb Strength, ksi [MPa] Produc onium Base Alloys [mm] Diameter Diameter .2 (Continued) Thickness or (Continued) Limitations, in in Limitations, 702[380/205] 55/30 Bar & Wire 99.2Zr Table C 0702 55/30 [380/205] Forgings 99.2Zr UNS Number Zirconium and Zirc Zirconium Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 6161 6161 6161 61 ASTM 61 ASTM61 ASTM61 B351 ASTM 6161 B351 6161 B351 R60001 6161 B353 ASTM R60802 6161 ASTM R60001 R60804 6161 ASTM R60802 R60001 6161 B352 ASTM/ASME ASTM R60804 6161 B353 ASTM/ASME B/SB-493 R60001 6161 B353 ASTM/ASME B/SB-523 R60804 61 B353 ASTM/ASME B/SB-550 R60702 R60001 61 ASTM/ASME B/SB-551 R60702 R60804 R60802 ASTM/ASME R6 B/SB-653 R60702 42/20 [290/140] R60001 R60804 R60702 B/SB-658 R60702 60/35 [415/240] R60802 R60 R60702 60/35 [415/240] Rod, & Wire Bar, R60804 R60702 R60702 42/20 [290/ Bar, R60702 Bar, R60702 58/35 [400/240] 99.9Zr [290/140] 42/20 [380/205] 55/30 Tube Seamless & Welded 60/35 [415/240]Tube Seamless & Welded Seamle 60/35 [415/240] 55/30 Plate Seamle 55/30 [ 55/30 99.9Zr 99.2Zr 98.2Zr-1.5Sn-0.32(Fe+Cr) 6161 61 61 ASTM ASTM B352 B352 R60802 R60804 R6080262 R6080462 62 62 ASTM ASTM 58/35 [400/240] B351 56/35 [385/240] B352 Plate, R60901 Sh R60901 R60901 R60901 65/45 [450/310] 65/45 [450/310] Rod, & Wire Bar, Pl 97.3Zr-2.6Cb 6262 6262 6262 6262 ASTM 6262 ASTM/ASME ASTM 6262 ASTM/ASME B/SB-493 6262 B353 ASTM/ASME B/SB-493 6262 B353 ASTM/ASME B/SB-523 R60704 62 ASTM/ASME B/SB-523 R60705 R60901 62 ASTM/ASME R60704 B/SB-550 R60704 R60904 ASTM/ASME R60705 B/SB-550 R60705 R60901 R60704 B/SB-551 R60704 R60904 R60705 R60705 R60704 R60704 R60705 R60704 60/35 [450/310] 65/45 60/35 [415/240]Tube Seamless & Welded [450/310] 65/45 Se 80/55 [ Tube Seamless & Welded 60/35 [ 97.3Zr-2.6Cb 97.35Zr-2.65Cb 60/35 [415/240] Pl 6262 62 62 ASTM/ASME ASTM/ASME B/SB-551 B/SB-551 R60705 R60706 R60705 R60706 80/55 [550/ 74/50 [510/ Material Number
199 AWS B2.1/B2.1M-BMG:2014 97.5Zr-1.5Sn-0.3(Fe+Cr) Pipe 95.5Zr+2.5Cb t Form Nominal Composition amless & Welded Pipe amless & Welded 380] Seamless & Welded Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc onium Base Alloys [mm] Diameter Diameter .2 (Continued) Thickness or Limitations, in in Limitations, Table C UNS Number Zirconium and Zirc Zirconium Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 62 62 ASTM/ASME B/SB-658 R60705 R60705 80/55 [550/ 62 62 ASTM/ASME B/SB-658 R60704 R60704 60/35 [415/240] Se Material Number
200 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition Plate & Sheet 95.5Mg-3Al-Zn-Mn r, Rods, Profiles, & Wire Rods, Profiles, r, 95.5Mg-3Al-Zn-Mn Minimum Minimum Tensile/Yield Tensile/Yield 29/14 [200/97] Plate 95.5Mg-3Al-Zn 29/12 [200/83] Plate 98Mg-1.25Zn-0.17Re 29/13 [200/90] Tube 95.5Mg-3Al-Zn-Mn 30/15 [205/105] Sheet 98Mg-1.25Zn-0.17Re 30/18 [205/125] Sheet 98Mg-1.25Zn-0.17Re 32/18 [220/125]30/15 [205/105] Sheet Plate 95.5Mg-3Al-Zn 95.5Mg-3Al-Zn 30/16 [205/110]30/16 Plate & Sheet 95.5Mg-3Al-Zn 32/15 [220/105]32/15 Plate & Sheet 95.5Mg-3Al-Zn 29/17 [200/115] & Wire Rods, Profiles, Bar, 95.5Mg-3Al-Zn-Mn 31/19 [215/130] & Wire Rods, Profiles, Bar, 95.5Mg-3Al-Zn-Mn 29/17 [200/115] Tube 95.5Mg-3Al-Zn-Mn 32/19 [220/130] & Wire Rods, Profiles, Bar, 95.5Mg-3Al-Zn-Mn Strength, ksi [MPa] Produc 3 0.5 6] 1 0.06 0.06 0.5 0.25 13] 80] ≤ 0.25 25] 3 80] 0.75 1.5] 1.5] 6] ≤ ≤ ≤ 20] 13] ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ esium Base Alloys Base esium [mm] 1 and 1 6 and 6 and <40] 2.5 and <5 2.5 Diameter Diameter 40 and <60] 40 ≥ 0.4 and 1.5 and 0.06 and 0.4 and 0.4 0.4 and 0.4 60 and <130] 1.5 and <2.5 ≥ ≥ [ ≥ .2 (Continued) 0.25 and 0.25 and <1.5 ≥ Thickness or [ [ [>6 and ≥ ≥ ≥ 0.016 and 0.016 [>1.5 and [>1.5 and ≥ ≥ ≥ ≥ [>13 and [>13 and [>25 and [ (Continued) Limitations, in in Limitations, 0.016 and 0.016 and 0.028 and [ [ ≥ ≥ [ [ [ ≥ ≥ ≥ ≥ Table C UNS Number Magnesium and Magn Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 81 — ASTM B91 AZ31B M11311 32/15 [220/105] Forgings 95.5Mg-3Al-Zn-Mn 81 — ASTM B90 ZE10A M16100 >0.06 and 81 —81 ASTM81 — — B90 ASTM ASTM HK31A B90 M13310 B90 HK31A ZE10A M13310 M16100 >1 and 81 — ASTM81 — B90 ASTM HK31A M13310 B90 >0.5 and ZE10A M16100 81 — ASTM B90 AZ31C M11312 8181 — — ASTM ASTM B90 B90 AZ31B AZ31C M11311 M11312 [220/–] 32/– 8181 — — ASTM ASTM B107 B107 AZ31B AZ31B M11311 M11311 <0.25 [<6] 32/18 [220/125] Ba 8181 — — ASTM ASTM B107 B107 AZ31B AZ31B M11311 M11311 29/13 [200/90] Profiles Hollow 95.5Mg-3Al-Zn-Mn 8181 — — ASTM ASTM B91 B107 AZ61A AZ31B M11610 M11311 35/19 [240/130] Forgings 92.5Mg-6Al-Zn 8181 — — ASTM ASTM B107 B107 AZ31B AZ31B M11311 >0.25 and M11311 Material Number
201 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition r, Rods, Profiles, & Wire Rods, Profiles, r, 92.5Mg-6Al-Zn r, Rods, Profiles, & Wire Rods, Profiles, r, 95.5Mg-3Al-Zn 125] & Wire Rods, Profiles, Bar, 98Mg-Mn Minimum Minimum Tensile/Yield Tensile/Yield 33/13 [230/90] Tube 92.5Mg-6Al-Zn 33/13 [230/90] Tube 98Mg-Mn 29/13 [200/90] Tube 95.5Mg-3Al-Zn 37/19 [255/130] & Wire Rods, Profiles, Bar, 92.5Mg-6Al-Zn 37/21 [255/145] & Wire Rods, Profiles, Bar, 92.5Mg-6Al-Zn 29/17 [200/115] Tube 95.5Mg-3Al-Zn 31/19 [215/130] & Wire Rods, Profiles, Bar, 95.5Mg-3Al-Zn 37/19 [255/130] & Wire Rods, Profiles, Bar, 98Mg-Mn 37/21 [255/145] & Wire Rods, Profiles, Bar, 98Mg-Mn 29/17 [200/115] & Wire Rods, Profiles, Bar, 95.5Mg-3Al-Zn 32/19 [220/130] & Wire Rods, Profiles, Bar, 95.5Mg-3Al-Zn Strength, ksi [MPa] Produc 0.75 0.75 0.25 0.25 0.75 6] 20] 20] 20] ≤ ≤ ≤ ≤ ≤ ≤ ≤ ≤ esium Base Alloys Base esium [mm] 1 and 1 1 and 1 and 6 and <60] 6 and <60] 6 and <40] 2.5 and <5 2.5 2.5 and <5 2.5 2.5 and <5 2.5 Diameter Diameter 40 and <60] 40 ≥ 60 and <130] 60 and <130] 60 and <130] 1.5 and <2.5 ≥ ≥ ≥ ≥ ≥ [ ≥ ≥ ≥ .2 (Continued) 0.25 and <2.5 0.25 and <2.5 0.25 and <1.5 ≥ Thickness or [ [ [ [>6 and [ [ ≥ ≥ ≥ ≥ [ (Continued) Limitations, in in Limitations, 0.028 and 0.028 and 0.028 and ≥ ≥ ≥ [ [ [ ≥ ≥ ≥ Table C UNS Number Magnesium and Magn Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 81 — ASTM B107 AZ61A M11610 8383 —83 — — ASTM ASTM ASTM B80 B80 B80 AZ91C, F AZ92A, F M11914 M11920 K1A M18010 21/10 [145/69][145/69] 21/10 Castings 22/5 [150/34] Castings Castings 90.5Mg-9Al-Zn-Mn 88.5Mg-9Al-2Zn-Mn 99.6Mg-Zr 8181 —81 — — ASTM ASTM ASTM B107 B107 B107 M1A M1A M1A M15100 M15100 M15100 <0.25 [<6] 35/18 [240/ 33/13 [230/90] Profiles Hollow 98Mg-Mn 81 — ASTM B107 AZ61A M11610 81 — ASTM B107 AZ61A M11610 <0.25 [<6] 35/18 [240/125] Ba 8181 — — ASTM ASTM B107 B107 AZ61A AZ61A M11610 M11610 33/13 [230/90] Profiles Hollow 92.5Mg-6Al-Zn 8181 —81 — ASTM — ASTM ASTM B107 B107 AZ31C B107 AZ31C M11312 AZ31C >0.25 and M11312 M11312 <0.25 [<6] 32/18 [220/125] Ba 81 — ASTM B107 M1A M15100 81 — ASTM B107 M1A M15100 8181 — — ASTM ASTM B107 B107 AZ31C AZ31C M11312 M11312 29/13 [200/90] Profiles Hollow 95.5Mg-3Al-Zn 81 — ASTM B107 AZ31C M11312 81 — ASTM B107 AZ31C M11312 Material Number
202 AWS B2.1/B2.1M-BMG:2014 t Form Nominal Composition 125/62] Castings 88.5Mg-9Al-2Zn-Mn Minimum Minimum Tensile/Yield Tensile/Yield Strength, ksi [MPa] Produc esium Base Alloys Base esium [mm] Diameter Diameter .2 (Continued) Thickness or Limitations, in in Limitations, Table C UNS Number Magnesium and Magn Alloy Alloy Designation Type, Grade, or Grade, or Type, Base Metal Metal Base Specification M-Number Listing of Base Metals—Nonferrous Alloys (see C.1, I2.2.1, and I3) and C.1, I2.2.1, (see Alloys of Base Metals—Nonferrous Listing M-Number ISO 15608 15608 Group Standard 83 — ASTM B403 K1A M18010 22/5 [150/34] Castings 99.6Mg-Zr 8383 —83 —83 —83 ASTM —83 ASTM — ASTM — B199 ASTM B199 ASTM B199 ASTM AM100A B403 F AZ91C, B403 M10100 F AZ92A, M11914 B403 F AM100A, M11920 F AZ91C, M10100 F AZ92A, M11914 M11920 18/9 [125/62] 21/10 [145/69][145/69] 21/10 [125/62] 18/9 Castings 16/9 [110/62] Castings[ 18/9 Castings Castings Castings 89.5Mg-10Al-Mn 90.5Mg-9Al-Zn-Mn 88.5Mg-9Al-2Zn-Mn 89.5Mg-10Al-Mn 90.5Mg-9Al-Zn-Mn Material Number
203 AWS B2.1/B2.1M-BMG:2014
Table C.3 Listing of Base Metal Specifications—Iron Castings
Minimum As-Welded AWS Type, Grade, Tensile/Yield D11.2 Base Metal or Alloy UNS Strength, Type of Nominal Group Standard Specification Designation Number ksi [MPa] Base Metal Composition Iron Castingsa, b A ASTM A48 Class 20 F11401 20/– [138/–] Gray Cast Iron Not Specified A ASTM A48 Class 25 F11701 25/– [172/–] Gray Cast Iron Not Specified A ASTM A48 Class 30 F12101 30/– [207/–] Gray Cast Iron Not Specified A ASTM A48 Class 35 F12401 35/– [241/–] Gray Cast Iron Not Specified A ASTM A48 Class 40 F12801 40/– [276/–] Gray Cast Iron Not Specified A ASTM A48 Class 45 F13101 45/– [310/–] Gray Cast Iron Not Specified A ASTM A48 Class 50 F13501 50/– [345/–] Gray Cast Iron Not Specified A ASTM A48 Class 55 F13801 55/– [379/–] Gray Cast Iron Not Specified A ASTM A48 Class 60 F14101 60/– [414/–] Gray Cast Iron Not Specified A ASTM A74 Class A — 21/– [145/–] Gray Cast Iron 0.75 Max.P, 0.15 Max.S A ASTM A126 Class A F11501 21/– [145/–] Gray Cast Iron 0.75 Max.P, 0.15 Max.S A ASTM A126 Class B F12102 31/– [214/–] Gray Cast Iron 0.75 Max.P, 0.15 Max.S A ASTM A126 Class C F12103 41/– [283/–] Gray Cast Iron 0.75 Max.P, 0.15 Max.S A ASTM A159 Grade 1800 F10004 18/– [124/–] Gray Cast Iron 0.55Si-0.65Mn; 4.35CE A ASTM A159 Grade 2500 F10005 25/– [172/–] Gray Cast Iron 2.2 Si-0.75Mn; 4.12CE A ASTM A159 Grade 2500a F10009 25/– [172/–] Gray Cast Iron 1.85Si-0.75Mn; 4.12 CE A ASTM A159 Grade 3000 F10006 30/– [207/–] Gray Cast Iron 2.1Si-0/75Mn; 4.02CE A ASTM A159 Grade 3500 F10007 35/– [241/–] Gray Cast Iron 2.0Si-0.75Mn; 3.8CE A ASTM A159 Grade 3500b F10010 35/– [241/–] Gray Cast Iron 1.55Si-0.75Mn; 3.8CE A ASTM A159 Grade 3500c F10011 35/– [241/–] Gray Cast Iron 1.55Si-0.75Mn; 3.8CE A ASTM A159 Grade 4000 F10008 40/– [276/–] Gray Cast Iron 1.95Si-0.85Mn; 3.8CE A ASTM A159 Grade 4000d F10012 40/– [276/–] Gray Cast Iron 1.95Si-0.85Mn; 3.8CE A ASTM A319 Class I F10001 25/– [172/–] Gray Cast Iron Not Specified A ASTM A319 Class II F10002 30/– [207/–] Gray Cast Iron Not Specified A ASTM A319 Class III F10003 40/– [276/–] Gray Cast Iron Not Specified A SAE J431 G1800 F10004 18/– [124/–] Gray Cast Iron 2.3SI-0.65Mn; 4.35CE A SAE J431 G2500 F10005 25 [172] Gray Cast Iron 2.3Si-0.75Mn; 4.12CE A SAE J431 G3000 F10006 30 [207] Gray Cast Iron 2.1Si-0.65Mn; 4.02CE A SAE J431 G3500 F10007 35 [241] Gray Cast Iron 2.0Si-0.75Mn; 3.8CE A SAE J431 G4000 F10008 40 [276] Gray Cast Iron 1.95Si-0.95Mn; 3.8CE
B ASTM A536 100-70-03 F34800 100/70 [689/483] Ductile Not Specified B ASTM A536 120-90-02 F36200 120/90 [827/621] Ductile Not Specified B ASTM A536 60-40-18 F32800 60/40 [414/276] Ductile Not Specified B ASTM A536 65-45-12 F33100 65/42 [448/290] Ductile Not Specified B ASTM A536 80-55-06 F33800 80/55 [552/379] Ductile Not Specified B ASTM A716 60-42-10 F32900 60/– [414/–] Ductile Not Specified B ASTM A746 60-42-10 — 60/– [414/–] Ductile Not Specified B ASTM A874 — — 45/30 [310/207] Ductile 3.35C-1.75Si B ASTM A897 125-80-10 — 125/80 [862/552] Ductile 1.0Ni-0.5Cu-0.35Mn-0.015Mo B SAE J434 D4018 F32800 60/– [414/–] Ductile Not Specified
204 AWS B2.1/B2.1M-BMG:2014
Table C.3 (Continued) Listing of Base Metal Specifications—Iron Castings
Minimum As-Welded AWS Type, Grade, Tensile/Yield D11.2 Base Metal or Alloy UNS Strength, Type of Nominal Group Standard Specification Designation Number ksi [MPa] Base Metal Composition Iron Castingsa, b B SAE J434 D4512 F33100 65/– [448/–] Ductile Not Specified B SAE J434 D5506 F33800 80/– [552/–] Ductile Not Specified B SAE J434 D7003 F34800 100/– [689/–] Ductile Not Specified
C ASTM A47 32510 F22200 50/– [345/–] Malleable Not Specified C ASTM A47 35018 F22400 53/– [365/–] Malleable Not Specified C ASTM A197 — F22200 40/– [276/–] Malleable Not Specified C ASTM A220 40010 F22830 60/– [414/–] Malleable Not Specified C ASTM A220 45006 F23131 65/– [448/–] Malleable Not Specified C ASTM A220 45008 F23130 65/– [448/–] Malleable Not Specified C ASTM A220 50005 F23530 70/– [483/–] Malleable Not Specified C ASTM A220 60004 F24130 80/– [552/–] Malleable Not Specified C ASTM A220 70003 F24830 85/– [586/–] Malleable Not Specified C ASTM A220 80002 F25530 95/– [655/–] Malleable Not Specified C ASTM A220 90001 F26230 105/– [724/–] Malleable Not Specified C ASTM A602 M3210 F20000 50/– [345/–] Malleable Not Specified C ASTM A602 M4504 F20000 65/– [448/–] Malleable Not Specified C ASTM A602 M5003 F20000 75/– [517/–] Malleable Not Specified C SAE J158a M3210 F20000 50/– [345/–] Malleable Not Specified C SAE J158a M4504 F20001 65/– [448/–] Malleable Not Specified a In the absence of an M number to group the alloys, a separate procedure qualification is required for each group of the above materials. b The groups are based on AWS D11.2.
205 AWS B2.1/B2.1M-BMG:2014
This page is intentionally blank.
206